Parameter determination method and application of stress relaxation model for shield tunnel aging gasket
Through the accelerated aging test and the time-temperature conversion relationship established by the Arrhenius equation, combined with the Mooney-Rivlin model, the stress relaxation simulation problem of the shield tunnel rubber sealing gasket in the complex pre-compression state was solved, and the shield tunnel rubber seal was realized. The long-term service performance prediction of the seal improves the waterproof design and operational safety of shield tunnels.
Patent Information
- Application Number
- CN202410052575.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-01-15
AI Technical Summary
Existing technology is difficult to accurately simulate the stress relaxation effect of shield tunnel rubber seals in long-term service, especially under complex pre-compression strain conditions. It cannot effectively predict its waterproof performance, and it is difficult to obtain existing model parameters and is not suitable for application. Wide applicability.
The parameters of the rubber constitutive model are obtained through accelerated aging tests, and the Arrhenius equation is used to establish the time-temperature conversion relationship. Combined with the Mooney-Rivlin model, the stress relaxation simulation of the rubber sealing gasket in the pre-compression state is realized and the time-varying model parameters are provided. , directly used in finite element software to simulate the long-term service state of rubber seals.
It realizes the simulation of the stress relaxation characteristics of the shield tunnel rubber seal under complex pre-compression state, provides the ability to predict long-term service performance, improves the accuracy of shield tunnel waterproof design and operational safety, and reduces maintenance and economic losses. risk.
Smart Images

Figure CN117871259B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of shield tunnel waterproof sealing pads, and in particular to a method for determining parameters of a stress relaxation model of an aging sealing pad for a shield tunnel and an application thereof. Background Art
[0002] With the rapid development of my country's economy and the advancement of construction technology, the shield method has been widely used in the construction of urban underground railways and cross-sea and cross-river tunnels due to its advantages of safe construction, fast excavation speed, and high degree of automation. The rubber elastic sealing pad is the main body of the shield tunnel joint waterproofing system. Its working principle is to compress the elastic sealing pad tightly and close it through the shield jack to generate contact stress to resist the intrusion of external water pressure. However, with the increase of service time, the rubber sealing pad will inevitably produce stress relaxation, which will increase the risk of tunnel leakage. In addition, the shield sealing pad used in actual engineering is a porous and complex structure. For a certain pre-compression amount, its strain is not uniform. On the entire cross section, some parts have large strains and some parts have small strains. The uneven strain distribution of the sealing pad brings great difficulties to the research of rubber sealing pads. Therefore, accurately simulating the long-term stress relaxation effect of rubber sealing pads is crucial for the waterproof design of shield tunnels.
[0003] Finite element software is usually used to simulate the waterproof ability of rubber gaskets, and the simulated compression force or surface contact stress of the gasket is used as an indicator to measure its waterproof ability. Xue Guangqiao et al. (Xue Guangqiao, Yu Xiongbing, Xiao Mingqing, Zhang Chaoyong, He Yingdao. Numerical simulation of waterproof performance of gaskets considering compression-staggered joints-external water pressure [J]. Modern Tunnel Technology, 2023, 60(03): 139-145+174) used the Mooney-Rivlin constitutive model to numerically simulate the compression performance of rubber gaskets and studied the contact stress distribution of rubber gaskets under various working conditions. However, this study has the following characteristics or limitations: the parameters of its rubber constitutive model are selected according to empirical formulas, so the performance of rubber gaskets after aging cannot be simulated.
[0004] Artificial accelerated aging test is a common method to study the long-term service performance of rubber materials. Ding Wenqi et al. (Ding Wenqi, Zhao Wei, Peng Yicheng, Guo Xiaohong, Yang Linsong, Tuo Yongfei. Research on the prediction method of long-term waterproof performance of shield tunnel waterproof seals [C] / / Collection of underwater tunnel construction and management technology. 2013:6) conducted an accelerated aging test on rubber cylindrical specimens with a pre-compression strain of -0.3, and used the stress relaxation coefficient as a performance index to predict the long-term stress relaxation of rubber seals using the Arrhenius equation. However, this study has the following characteristics or limitations: the rubber seals in the project are porous structures, and the pre-compression strain on the cross section of the seal under working conditions is unevenly distributed, rather than a constant value. This study only selected the pre-compression strain of -0.3 for research, which cannot accurately describe the stress relaxation effect of tunnel seals under complex pre-compression strain states.
[0005] For the stress relaxation constitutive model of rubber, patent document CN112199823B (application date September 17, 2020, publication date January 8, 2021) provides a numerical prediction method for the stress relaxation effect of rubber materials. First, hyperelastic mechanical tests and stress relaxation tests of rubber materials are carried out, and then the proposed time-varying relaxation-damage constitutive model is embedded in commercial finite element software using the UHYPER subroutine written in Fortran language. The material constitutive parameters are identified using a multi-island genetic algorithm, and finally the simulation of the time-varying relaxation effect of rubber materials is realized. This study has the following characteristics or limitations: 1) The proposed constitutive model requires secondary development of commercial finite element software, which requires relevant programming knowledge and is difficult to apply; 2) The acquisition of model parameters requires the use of a multi-island genetic algorithm to continuously write new parameters into the constitutive model until the simulation results meet the accuracy requirements, which makes it difficult to obtain its constitutive parameters.
[0006] In summary, the current shield tunnel sealing gasket aging stress relaxation simulation technology has the following limitations:
[0007] 1) Existing studies usually obtain rubber constitutive model parameters based on empirical formulas or test curve fitting, and input them into finite element software for analysis. However, these two methods can only be used to characterize the properties of unaged rubber materials and cannot predict the long-term service performance of rubber materials.
[0008] 2) Most accelerated aging tests set a single pre-compression strain, while shield tunnel gaskets in actual service are often in a complex pre-compression strain state. The rubber stress relaxation law obtained from the test is not applicable to the service conditions of the gaskets.
[0009] 3) The model parameters of some complex stress relaxation constitutive models are difficult to obtain and need to be obtained with the help of algorithms and simulation iterations. The application of these models requires secondary development of finite element software by coding subroutines, which does not have wide applicability.
[0010] Therefore, it is necessary to propose a method for determining the parameters of the stress relaxation model of shield tunnel aging gaskets under complex strain states and its application, so as to predict the long-term service performance of rubber gaskets and provide a basis for the design of long-term waterproof capacity of shield tunnels. Summary of the invention
[0011] The purpose of the present invention is to provide a method for determining parameters of a stress relaxation model of a rubber aging sealing pad of a shield tunnel under a pre-compression state and its application, so as to solve the above technical problems.
[0012] The basic principle of the present invention is: firstly, an accelerated aging test is performed on a pre-compressed rubber material cylindrical sample to obtain rubber constitutive model parameters that characterize the stress relaxation characteristics of the pre-compression state; based on the Arrhenius equation, the time-temperature conversion relationship between the test working condition and the actual service state of the rubber sample is obtained, and then the time-varying law of the rubber stress relaxation constitutive model parameters is obtained; when applied, the obtained constitutive model parameters are input into a finite element model to realize the simulation of the long-term service stress relaxation characteristics of the aged sealing gasket in the pre-compression state.
[0013] To achieve the above object, the present invention adopts the following technical solution:
[0014] The present invention provides a method for determining parameters of a stress relaxation model of an aging sealing gasket in a shield tunnel, comprising the following steps:
[0015] Step 1: setting different test conditions, conducting accelerated aging tests under pre-compression on rubber samples with the same material and processing technology as the rubber sealing pad of the shield tunnel, and obtaining aged rubber samples under different test conditions; the test conditions include pre-compression strain, aging temperature and aging time;
[0016] It should be noted that in the accelerated aging test described in step 1, the rubber sample is a cylindrical sample, the pre-compression strain range of the rubber sample is 0 to E, E is the maximum pre-compression strain, E is -0.4 to -0.6, preferably -0.4, at least 5 different pre-compression strains are set, and the interval between different pre-compression strains is less than or equal to -0.1 to ensure the fitting accuracy of the stress relaxation constitutive model; at least 3 different aging temperatures are set under each pre-compression strain, the selection range of the aging temperature is 55°C to 100°C, and the interval of the aging temperature is preferably 10 to 20°C; at least 5 different aging times are set under each aging temperature, and the aging time is generally selected as a multiple of 24h.
[0017] Step 2: Using an electronic universal testing machine, perform uniaxial compression tests on the unaged rubber sample and the aged rubber samples under different test conditions described in step 1 to obtain compression stress-strain curves of the unaged rubber sample and each aged rubber sample;
[0018] Step 3: taking the ratio of the stress of the aged rubber sample at the pre-compression strain to the stress of the unaged rubber sample at the same strain as the stress relaxation coefficient, calculating the average stress relaxation coefficient of the aged rubber sample at different pre-compression strains according to the compression stress-strain curves of the unaged rubber sample and each aged rubber sample obtained in step 2, establishing an accelerated aging model with the average stress relaxation coefficient as a performance index according to the time-temperature equivalence theory and fitting to obtain a reaction constant, establishing a time-temperature conversion relationship of the aged rubber sample using the Arrhenius equation according to the reaction constant in the accelerated aging model, and converting the aging temperature and aging time of the aged rubber sample in the accelerated aging test into the service time in the actual service state according to the time-temperature conversion relationship;
[0019] It should be noted that in step 3, the average stress relaxation coefficient at different pre-compression strains is determined according to formula (3.1):
[0020]
[0021] In the formula, is the average stress relaxation coefficient; K Ri is the stress relaxation coefficient of the aged rubber sample at the i-th pre-compression strain; σ 0i is the stress of the unaged rubber specimen at the i-th pre-compression strain, σ 1i is the stress of the aged rubber specimen at the i-th pre-compression strain; i = 1, 2, ..., n, where n is the number of pre-compression strains selected in the accelerated aging test.
[0022] It should be noted that in step 3, according to the time-temperature equivalence theory, the accelerated aging model with the average stress relaxation coefficient as the performance index is established according to formula (3.2):
[0023]
[0024] Wherein, B, K, α are reaction constants; t is the rubber aging time or service time, (h); and e is the natural logarithm constant.
[0025] It should be noted that in step 3, based on the reaction constant α in the accelerated aging model, the Arrhenius equation is used to establish the time-temperature conversion relationship of the aged rubber sample as shown in formula (3.3):
[0026]
[0027] Where, T 1is the aging temperature of the rubber sample during the accelerated aging test, (K); T 2 is the service temperature of the rubber gasket in actual service state, (K); t 1 is the aging time of the rubber sample in the accelerated aging test, (h); t 2 is the service time of the rubber gasket in actual service state, (h); E is the apparent activation energy, (J·mol -1 );R is the gas constant, (J·K -1 ·mol -1 ).
[0028] Step 4: grouping the compression stress-strain curves of the aged rubber sample obtained in step 2 according to the service time converted in step 3, determining a compression stress-strain curve group with the same service time, interpolating two adjacent compression stress-strain curves with different pre-compression strains in the compression stress-strain curve group according to the pre-compression strain, and obtaining a compression stress-strain curve with any pre-compression strain within the existing pre-compression strain range, and forming all compression stress-strain curves with the same service time into a compression stress-strain curve family; interpolating multiple compression stress-strain curve families with different service times of the aged rubber sample by the interpolation method; establishing a stress relaxation model based on the Mooney-Rivlin model for the aged rubber sample during the uniaxial compression test, fitting each compression stress-strain curve family to obtain stress relaxation model parameters corresponding to the service time, and establishing a time-varying relationship of the model parameters under the actual service state according to the model parameters of different service times;
[0029] It should be noted that in step 4, the inventors found in the uniaxial compression test process described in step 2 that the change trends of the compression stress-strain curve group of aged rubber samples with the same service time are basically the same. Therefore, the compression stress-strain curves of two adjacent different pre-compression strains in the compression stress-strain curve group are interpolated according to the pre-compression strain by using the interpolation method. The interpolation method uses the linear interpolation method to obtain the compression stress-strain curve of any pre-compression strain within the existing pre-compression strain range as shown in formula (4.1):
[0030]
[0031] Where σ(ε) i ,σ(ε) i+1 are the stresses of the aged rubber specimen at the i-th and i+1-th pre-compression strains respectively; σ(ε) i+k , ε p,i+k , ε c,i+kare the stress, pre-compression strain, and permanent strain of the aged rubber specimen at the i+kth pre-compression strain, respectively; m is the number of interpolation between the two compression stress-strain curves of the i-th and i+1-th pre-compression strains, and k is the number of the interpolation curve, k=1,2,3,...m-1;
[0032] The existing pre-compression strain range refers to the pre-compression strain range 0~Ε selected for the accelerated aging test;
[0033] Permanent strain refers to the irreversible deformation of an aged rubber specimen under pre-compression;
[0034] Among them, σ(ε) i ,σ(ε) i+1 , ε p,i+k , ε c,i+k Determine according to formula (4.2)~(4.4):
[0035]
[0036]
[0037]
[0038] In the formula, ε p,i , ε p,i+1 are the i-th and i+1-th pre-compression strains set in the uniaxial compression test respectively; ε c,i , ε c,i+1 The permanent strains of the aged rubber specimens at the i-th and i+1-th pre-compression strains were measured in the uniaxial compression test respectively.
[0039] It should be noted that in step 4, the stress relaxation model of the rubber sample in the uniaxial compression state is established based on the Mooney-Rivlin model according to formula (4.5):
[0040] σ=2(λ-λ -2 )C 10 +2(1-λ -3 )C 01 (4.5)
[0041] Where, σ is the stress of the aged rubber sample in the uniaxial compression state; λ is the elongation ratio of the aged rubber sample in the uniaxial compression state, λ = 1 + ε, ε is the strain of the aged rubber sample in the uniaxial compression state; C 10 , C 01 are the unknown parameters of the stress relaxation model.
[0042] It should be noted that in step 4, the inventors found during the research that the undetermined parameter C of the stress relaxation model 10 , C 01It has a good linear correlation with the natural logarithm of the service time; according to the model parameter C of different service time 10 , C 01 The time-varying relationship of the model parameters under actual service conditions is established according to formula (4.6):
[0043]
[0044] In the formula, m 10 , b 10 are the model parameters C 10 (t 2 ) fitting parameters of the time-varying relationship; m 01 , b 01 are the model parameters C 01 (t 2 ) fitting parameters of the time-varying relationship.
[0045] The method for determining stress relaxation model parameters of an aged sealing gasket in a shield tunnel described in the present invention, when applied, uses finite element software to establish an axial compression model of the sealing gasket, and uses the Mooney-Rivlin model in the finite element software to simulate the aged sealing gasket in a pre-compression state. According to the current service time of the aged sealing gasket in the actual service state, the corresponding stress relaxation model parameters are obtained according to the time-varying relationship of the model parameters in the actual service state such as formula (4.6). The model parameters are input into the finite element model, and after simulation calculation, the stress relaxation index of the aged sealing gasket in the actual service state under the pre-compression state (including the compression force and average contact stress of the aged sealing gasket) is obtained, and the waterproof ability of the aged sealing gasket at the current service time is determined according to the stress relaxation index.
[0046] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0047] 1) The stress relaxation constitutive model parameter determination method proposed in the present invention provides a time-varying relationship of the model parameters, and the corresponding model parameters can be obtained according to any service time. The model parameters can reflect the stress-strain relationship of the rubber sealing gasket of the shield tunnel after aging under any pre-compression strain, which provides a basis for the finite element simulation of the sealing gasket aged in a complex pre-compression state, and also provides ideas for the stress relaxation effect analysis of other rubber material products.
[0048] 2) The present invention interpolates the compressive stress-strain test curve to obtain the compressive stress-strain curve of the aged sealing gasket under any pre-compressive strain, and obtains the stress relaxation constitutive model parameters of the sealing gasket based on all the compressive stress-strain curves; using the Arrhenius equation, the time-varying law of the stress relaxation constitutive model parameters is obtained, and the constitutive parameters of the rubber sealing gasket material under any service time are predicted.
[0049] 3) The stress relaxation constitutive model proposed in the present invention is established based on the classic constitutive model of rubber materials. Therefore, it can be directly called in most commercial finite element software without writing subroutines to customize the constitutive model. It is convenient, efficient and practical.
[0050] 4) With the help of the time-varying expression of the Mooney-Rivlin model parameters under the actual service state proposed in the present invention, the model parameters of the same sealing gasket at any service time can be quickly obtained, which is helpful to realize the prediction of the long-term service performance of the shield sealing gasket, judge the waterproof performance of the shield sealing gasket in real time, improve the safety of shield tunnel operation, facilitate timely maintenance, reduce the risk of unexpected safety accidents and reduce unexpected economic losses. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 The present invention is a flow chart of the method for determining parameters of the stress relaxation model of an aging sealing pad in a shield tunnel and its application.
[0052] Figure 2 Schematic diagram of the strain of rubber specimens under different test conditions.
[0053] Figure 3 It is a schematic diagram of the shield rubber pad and the accelerated aging test sealing pad sample in Example 1; Figure (a) is a schematic diagram of the shield rubber pad, Figure (c) is a geometric dimension diagram of the shield rubber pad, and Figure (d) is a schematic diagram of the rubber sample.
[0054] Figure 4 Schematic diagram of the fitting curve of the average stress relaxation rate of the accelerated aging test in Example 1.
[0055] Figure 5 It is a schematic diagram of the interpolated compressive stress-strain curve of the rubber sample aged at 75°C for 48h in Example 1 and the fitting of the stress relaxation constitutive model.
[0056] Figure 6 C in Example 1 10 Parameter variation curve with service time.
[0057] Figure 7 C in Example 1 01 Parameter variation curve with service time.
[0058] Figure 8 This is the finite element model of the sealing gasket in Example 2.
[0059] Fig. 9 The stress cloud diagrams (unit: MPa) of the sealing gasket predicted to have a service life of 100 years in Example 2, FIG. (a) shows a seam opening amount Δ=0 mm, FIG. (b) shows a seam opening amount Δ=2 mm, and FIG. (c) shows a seam opening amount Δ=6 mm.
[0060] Fig.10 Schematic diagram of uniaxial loading of the unaged rubber sample in Example 2.
[0061] Fig.11 This is the compression force relaxation curve of the sealing gasket predicted to have a service life of 100 years in Example 2.
[0062] Fig.12 The results are a comparison of the compression force relaxation curves of the sealing gasket aged at 75°C for 48h by the uniaxial compression test and the finite element simulation in Example 2.
[0063] In the figure: σ is the stress on the rubber sample; σ 0i is the stress of the unaged rubber specimen at the i-th pre-compression strain, σ 1i is the stress of the aged rubber specimen at the i-th pre-compression strain; ε p,i is the i-th pre-compression strain set for the uniaxial compression test; ε c,i C is the permanent strain of the aged rubber sample at the i-th pre-compression strain measured in the uniaxial compression test; 10 , C 01 is the unknown parameter of the stress relaxation model (or Mooney-Rivlin model); Δ p is the pre-compression amount of the gasket. DETAILED DESCRIPTION
[0064] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention; it is obvious that the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0065] See also Figure 1-2 , Figure 1 It is a flow chart of the method for determining parameters of the stress relaxation model of the shield tunnel aging sealing pad of the present invention; Figure 2 Schematic diagram of the strain of rubber specimens under different test conditions.
[0066] The present invention provides a method for determining parameters of a stress relaxation model of an aging sealing gasket in a shield tunnel, comprising the following steps:
[0067] Step 1: setting different test conditions, conducting accelerated aging tests under pre-compression on rubber samples with the same material and processing technology as the rubber sealing pads of shield tunnels, and obtaining rubber samples after aging under different test conditions; the test conditions include pre-compression strain, aging temperature and aging time;
[0068] In the accelerated aging test, the rubber sample is a cylindrical sample. The pre-compression strain setting of the sample should try to cover the strain range of the shield sealing gasket when it is in service. According to the actual situation, it is generally selected to be 0 to -0.4. Since excessive pre-compression can easily lead to uneven compression and increase the experimental error, the maximum pre-compression strain is -0.6; therefore, the pre-compression strain range of the rubber sample is 0 to E, E is the maximum pre-compression strain, E is -0.4 to -0.6, preferably -0.4, at least 5 different pre-compression strains are set, and the interval between different pre-compression strains is less than or equal to -0.1 to ensure the fitting accuracy of the stress relaxation constitutive model; at least 3 different aging temperatures are set under each pre-compression strain, the selection range of the aging temperature is 55°C to 100°C, and the interval of the aging temperature is 10 to 20°C; at least 5 different aging times are set for each temperature condition, and the aging time is preferably a multiple of 24h, such as 24h, 48h, 96h, etc.
[0069] It should be noted that for the pre-compression strain range of 0~Ε, the endpoint values 0 and Ε are required pre-compression strain values, which can ensure the starting point and end point of the stress relaxation curve. Selecting a smaller pre-compression strain interval for the accelerated aging test can make the stress relaxation curve more representative. It is also convenient to use the interpolation method to obtain other characteristic points on the stress relaxation curve, making the fitting curve more accurate and reasonable. To a certain extent, it can improve the characterization accuracy of the model parameters, which is of great help in studying the strain distribution of aged sealing gaskets under complex pre-compression states.
[0070] The accelerated aging test of rubber samples is carried out according to Section 7 of GB / T 7759.1-2015 "Determination of compression set of vulcanized rubber or thermoplastic rubber". The height of the unaged rubber sample is h 0 , according to the height h of the center limiter of the fixture s Adjust the pre-compression strain of the sample, the compression amount of the rubber sample is h 0 -h s , then the pre-compression strain of the rubber sample is
[0071]
[0072] Step 2: Using an electronic universal testing machine, perform uniaxial compression tests on the unaged rubber sample and the aged rubber samples under different test conditions described in step 1, respectively, to obtain compression stress-strain curves (i.e., compression σ-ε curves) of the unaged rubber sample and each aged rubber sample;
[0073] After the accelerated aging test, the compression was immediately removed. After cooling at room temperature for 2 hours, the height of the rubber sample after aging was measured with a thickness gauge and the height h of the rubber sample after aging was recorded. 1 , then the permanent strain of the rubber sample is
[0074] The aged rubber sample was subjected to a uniaxial compression test using an electronic universal testing machine. The aged rubber sample was compressed to the pre-compression strain before aging. The compression amount is h 1 -h s ; Record the compressive stress-strain curve and the stress value σ when the aged rubber sample reaches the pre-compressive strain 1i .
[0075] Use an electronic universal testing machine to compress the unaged rubber sample and record the compression stress-strain curve and the stress value σ corresponding to the pre-compression strain. 0i .
[0076] Step 3: taking the ratio of the stress of the aged rubber sample at the pre-compression strain to the stress of the unaged rubber sample at the same strain as the stress relaxation coefficient, calculating the average stress relaxation coefficient of the aged rubber sample at different pre-compression strains according to the compression stress-strain curves of the unaged rubber sample and each aged rubber sample obtained in step 2, establishing an accelerated aging model with the average stress relaxation coefficient as a performance index according to the time-temperature equivalence theory and fitting to obtain a reaction constant, establishing a time-temperature conversion relationship of the aged rubber sample using the Arrhenius equation according to the reaction constant in the accelerated aging model, and converting the aging temperature and aging time of the aged rubber sample in the accelerated aging test into the service time in the actual service state according to the time-temperature conversion relationship;
[0077] It should be noted that the average stress relaxation coefficient at different pre-compression strains is determined according to formula (3.1):
[0078]
[0079] In the formula, is the average stress relaxation coefficient; K Ri is the stress relaxation coefficient of the aged rubber sample at the i-th pre-compression strain; σ 0i is the stress of the unaged rubber specimen at the i-th pre-compression strain, σ 1i is the stress of the aged rubber specimen at the i-th pre-compression strain; i = 1, 2, ..., n; n is the number of pre-compression strains selected in the accelerated aging test.
[0080] According to the time-temperature equivalence theory, the accelerated aging model with the average stress relaxation coefficient as the performance index is established according to formula (3.2):
[0081]
[0082] Wherein, B, K, α are reaction constants; t is the rubber aging time or service time, (h); and e is the natural logarithm constant.
[0083] According to the Arrhenius equation, the relationship between the chemical reaction rate and the aging temperature is:
[0084] lnK=lnA-E / RT (1)
[0085] Where K is the reaction constant; T is the absolute temperature, (K); E is the apparent activation energy, (J·mol -1 ); A is the frequency factor, R is the gas constant, (J·K -1 ·mol -1 ).
[0086] The aging temperature and aging time of the accelerated aging test are T 1 and t 1 , the service temperature and service time under actual service conditions are T 2 and t 2 , making the aging properties of the two equal, according to the reaction constant α in the accelerated aging model, the Arrhenius equation is used to establish the time-temperature conversion relationship of the aged rubber sample as shown in formula (3.3):
[0087]
[0088] Where, T 1 is the aging temperature of the rubber sample during the accelerated aging test, (K); T 2 is the service temperature of the rubber gasket in actual service state, (K); t 1 is the aging time of the rubber sample in the accelerated aging test, (h); t 2 is the service time of the rubber gasket in actual service status, (h);
[0089] Step 4: grouping the compression stress-strain curves of the aged rubber sample obtained in step 2 according to the service time converted in step 3, determining a compression stress-strain curve group with the same service time, interpolating two adjacent compression stress-strain curves with different pre-compression strains in the compression stress-strain curve group according to the pre-compression strain, and obtaining a compression stress-strain curve with any pre-compression strain within the existing pre-compression strain range, and forming all compression stress-strain curves with the same service time into a compression stress-strain curve family; interpolating multiple compression stress-strain curve families with different service times of the aged rubber sample by the interpolation method; establishing a stress relaxation model based on the Mooney-Rivlin model for the aged rubber sample during the uniaxial compression test, fitting each compression stress-strain curve family to obtain stress relaxation model parameters corresponding to the service time, and establishing a time-varying relationship of the model parameters under the actual service state according to the model parameters of different service times;
[0090] The inventors found that during the uniaxial compression test described in step 2, the change trends of the compression stress-strain curve group of aged rubber samples with the same service time are basically the same. Therefore, the compression stress-strain curves of two adjacent compression stress-strain curves with different pre-compression strains in the compression stress-strain curve group are interpolated according to the pre-compression strain respectively by using the interpolation method. The interpolation method uses the linear interpolation method to obtain the compression stress-strain curve of any pre-compression strain within the existing pre-compression strain range as shown in formula (4.1):
[0091]
[0092] Where σ(ε) i ,σ(ε) i+1 are the stresses of the aged rubber specimen at the i-th and i+1-th pre-compression strains respectively; σ(ε) i+k , ε p,i+k , ε c,i+k are the stress, pre-compression strain, and permanent strain of the aged rubber specimen at the i+kth pre-compression strain, respectively; m is the number of interpolation between the two compression stress-strain curves of the i-th and i+1-th pre-compression strains, and k is the number of the interpolation curve, k=1,2,3,...m-1;
[0093] The existing pre-compression strain range refers to the pre-compression strain range 0~Ε selected for the accelerated aging test;
[0094] Permanent strain refers to the irreversible deformation of an aged rubber specimen under pre-compression;
[0095] Among them, σ(ε) i ,σ(ε) i+1 , ε p,i+k , ε c,i+k Determine according to formula (4.2)~(4.4):
[0096]
[0097]
[0098]
[0099] In the formula, ε p,i , ε p,i+1 are the i-th and i+1-th pre-compression strains set in the uniaxial compression test respectively; ε c,i , ε c,i+1 The permanent strain of the aged rubber specimen at the i-th and i+1-th pre-compression strains were measured by uniaxial compression test respectively.
[0100] In other feasible implementations, other interpolation methods besides the linear interpolation method may also be used, but it is necessary to ensure that the error of the stress relaxation curve finally fitted is small.
[0101] The strain energy function expression of rubber hyperelastic material is:
[0102] W=W(I 1 ,I 2 ,I 3 ) (2)
[0103]
[0104] Where W is strain energy, I 1 , I 2 , I 3 is the tensor invariant, λ 1 ,λ 2 ,λ 3 Main elongation ratio.
[0105] The stress-strain relationship (stress relaxation constitutive model) of rubber materials in uniaxial compression tests is:
[0106]
[0107] Wherein, σ is the stress of the aged rubber sample in the uniaxial compression state; λ is the elongation ratio of the aged rubber sample in the uniaxial compression state, λ=1+ε, ε is the strain of the aged rubber sample in the uniaxial compression state;
[0108] The Mooney-Rivlin model is a classic rubber constitutive model based on continuum theory. It is the most widely used constitutive model for rubber materials because of its simple expression and easy to obtain parameters.
[0109] The strain energy function expression of the classic Mooney-Rivlin model is:
[0110] W=C 10 (I 1 -3)+C 01 (I 2 -3) (5)
[0111] Substituting formula (5) into formula (4), the stress relaxation model of the rubber sample based on the Mooney-Rivlin model in the uniaxial compression state is established according to formula (4.5):
[0112] σ=2(λ-λ -2 )C 10 +2(1-λ -3 )C 01 (4.5)
[0113] In the formula, C 10 , C 01 is the undetermined parameter of the stress relaxation model. 10 , C 01 That is, the undetermined parameters of the classic Mooney-Rivlin model.
[0114] The inventors found during the research that the undetermined parameter C of the stress relaxation model 10 , C 01 It has a good linear correlation with the natural logarithm of the service time; according to the model parameter C of different service time 10 , C 01 The time-varying relationship of the model parameters under actual service conditions is established according to formula (4.6):
[0115]
[0116] In the formula, m 10 、b 10 are the model parameters C 10 (t 2 ) fitting parameters of the time-varying relationship; m 01 、b 01 are the model parameters C 01 (t 2 ) fitting parameters of the time-varying relationship.
[0117] Since the design service life of shield tunnels in my country is currently 100 years, the aging temperature and aging time of the test conditions need to be specifically determined according to the converted service time, so that the service time converted from the test conditions can better represent the range of 0 to 100 years. 10 (t 2 )-ln(t 2 ) time-varying relation or C 01 (t 2 )-ln(t2 )Time-varying relationship.
[0118] The method for determining the model parameters of the aging stress relaxation of a shield tunnel sealing gasket described in the present invention, when applied, uses the Mooney-Rivlin model in the finite element software to simulate the aged sealing gasket in a pre-compression state, and obtains the corresponding stress relaxation model parameters according to the current service time of the aged sealing gasket in the actual service state and the time-varying relationship of the model parameters in the actual service state, such as formula (4.6). The model parameters are input into the finite element model, and the stress relaxation index (including the compression force and average contact stress of the aged sealing gasket) in the actual service state after being aged in the pre-compression state is obtained after simulation calculation, and the waterproof ability of the aged sealing gasket at the current service time is determined according to the stress relaxation index.
[0119] A large number of studies have shown that the compression force can reflect the waterproof ability of the gasket to a certain extent. For the aged gasket in the pre-compression state, the compression force decreases due to stress relaxation, and the waterproof ability also decreases accordingly. Therefore, this curve can provide a reference for the design of the long-term waterproof ability of the gasket.
[0120] Zhao Ming et al. (Zhao Ming, Ding Wenqi, Peng Yicheng, Shen Biwei, Guo Xiaohong, Yang Songlin. Experimental study on the reliability of waterproofing of high-pressure shield tunnel segment joints [J]. Modern Tunnel Technology, 2013, 50(03): 87-93) analyzed the results of the waterproofing performance test and compression test of the gasket and found that the average contact stress can fit the water pressure curve well and reflect the waterproofing ability of the gasket. Among them, the average contact stress can usually be calculated in the following two ways: the compression force obtained by the test or finite element simulation can be divided by the width of the gasket to approximate the average contact stress on the surface of the gasket; for finite element simulation, the contact stress distribution curve of the gasket surface path can also be extracted in post-processing, and then the average contact stress can be calculated. Therefore, the compression force and average contact stress of the aged gasket can reflect its long-term waterproofing performance.
[0121] It should be understood that compression force and average contact stress are a group of relatively reliable indicators for evaluating the waterproof ability of aged sealing gaskets in the prior art, but this does not mean that this embodiment is limited to the use of other evaluation indicators.
[0122] With the help of the time-varying relationship of the model parameters under the actual service state proposed by the present invention, technical personnel in this field can quickly obtain the model parameters of the same sealing gasket at any service time, thereby quickly and accurately realizing finite element modeling analysis of shield sealing gaskets, which is helpful to realize the prediction of the long-term service performance of shield sealing gaskets, judge the waterproof performance of shield sealing gaskets in real time, improve the safety of shield tunnel operation, facilitate timely maintenance, reduce the risk of unexpected safety accidents and reduce economic losses.
[0123] Embodiment 1;
[0124] See also Figure 1-7 ;
[0125] This embodiment provides a method for determining parameters of a stress relaxation model of an aging sealing gasket in a shield tunnel, specifically comprising the following steps:
[0126] According to step 1, in this embodiment, the pre-compression strain of the rubber sample is 0, -0.1, -0.2, -0.3, -0.4 respectively. The aging temperature is set to 55°C, 65°C, 75°C respectively, the aging time is set to 24h, 48h, 72h, 96h, 168h respectively, and the aging method adopts the hydrothermal aging test; Figure 3 Schematic diagram of the shield rubber pad and the accelerated aging test sealing pad sample in Example 1; Figure (a) is a schematic diagram of the shield rubber pad sealing pad, Figure (c) is a geometric dimension diagram of the shield rubber sealing pad, and Figure (d) is a schematic diagram of the rubber sample;
[0127] According to step 2, the compressive stress-strain curve of the unaged rubber sample is obtained, the compressive stress-strain curve of the aged rubber sample and the stress when the pre-compression strain is reached are obtained, and the compressive stress-strain curves of the unaged rubber sample and the 75℃-48h aged rubber sample are as follows: Figure 5 The electronic universal testing machine used is Mester CMT4104 electronic universal testing machine with a maximum range of 10kN, displacement controlled loading and a loading rate of 10mm / min.
[0128] According to step three, the average stress relaxation coefficient is calculated by formula (3.1), and the average stress relaxation coefficient curve of the rubber sample is fitted by formula (3.2). The fitting curve is as follows: Figure 4 ;
[0129] The reaction constants at different aging temperatures were obtained by fitting, as shown in Table 1.
[0130] Table 1 Reaction constants at different aging temperatures
[0131]
[0132] Substituting the data in Table 1 into the Arrhenius equation (1), the following parameters are obtained: lnA = 8.9331, E / R = 3825.74.
[0133] From (3.3), the time-temperature conversion relationship of the uniaxial compression test condition can be obtained as follows: The converted service time under actual service conditions is shown in Table 2. Table 2 Time-temperature conversion relationship between test conditions and service conditions
[0134]
[0135]
[0136] According to step 4, the experiment measured ε p =The stress relaxation curves under four specific pre-compression strains are: =-0.1, -0.2, -0.3, -0.4. Ten equal parts of linear interpolation are performed between every two test curves (m is 10). The expression of the interpolated compressive stress-strain curve is calculated by equations (4.1)-(4.4). The interpolated compressive stress-strain curve and the stress relaxation constitutive model fitting diagram of the rubber specimen aged at 75℃-48h are shown in Figure 5 The end point of the interpolated curve (relaxation stress) can reflect the stress relaxation characteristics of aged rubber specimens under different pre-compression strains.
[0137] The end point (relaxation stress) of the interpolated compressive stress-strain curve is fitted using formula (4.5) to obtain the stress relaxation model parameter C of each aged rubber sample. 10 , C 01 .
[0138] According to the service time of the rubber sample from the accelerated aging test state to the actual service state obtained in Table 2, the stress relaxation model parameter C is fitted using formula (4.6) 10 , C 01 The time-varying relationship of Figure 6 , 7 , Figure 5 C 10 Parameter variation curve with service time, Figure 7 C 01 The parameter variation curve with service time is fitted in this embodiment: C 10 (t 2 )=-0.155ln(t 2 )+2.613,C 01 (t 2 )=0.032ln(t 2 )-0.519, fitting correlation coefficient R 2 They are 0.974 and 0.986 respectively, indicating that the fitting effect is very good.
[0139] Embodiment 2;
[0140] See also Figure 8-12 ;
[0141] When applying the method for determining the model parameters of shield tunnel sealing gasket aging stress relaxation described in this embodiment, a commercial finite element software is used to establish an axial compression model of the sealing gasket, and the Mooney-Rivlin model is used in the finite element software to simulate the aged sealing gasket in a pre-compression state. According to the current service time of the aged sealing gasket in the actual service state, the corresponding stress relaxation model parameters are obtained according to the time-varying relationship of the model parameters in the actual service state such as formula (4.6). The model parameters are input into the finite element model, and the stress relaxation characteristics of the aged sealing gasket in the actual service state after simulation and calculation (including the compression force and average contact stress of the aged sealing gasket) in the pre-compression state are obtained. According to the stress relaxation characteristics, the waterproof ability of the aged sealing gasket at the current service time is determined.
[0142] The finite element modeling process is a conventional technical means in this field and will not be described in detail here.
[0143] This embodiment relies on the model parameter C established in Embodiment 1 10 , C 01 The time-varying relationship under actual service conditions, the specific simulation analysis process is as follows:
[0144] The gasket is selected with the same cross section as the actual service state gasket. The gasket is simulated by two-dimensional solid element, the segment groove is simulated by analytical rigid body, and the spacing between the upper and lower segment grooves is defined as the joint opening Δ. Dynamic explicit analysis is adopted, and the element type is selected as CPS4R four-node bilinear plane stress quadrilateral element, such as Figure 8 ;
[0145] The constitutive model of the sealing gasket is the Mooney-Rivlin constitutive model, and the service time t 2 =876000h (100 years) Substitute into the formula C obtained in Example 1 10 (t 2 )=-0.155ln(t 2 )+2.613、C 01 (t 2 )=0.032ln(t 2 )-0.519, the constitutive parameter C is calculated 10 =0.492, C 01 =-0.081.
[0146] Fig. 9 The stress-strain cloud diagram of the sealing gasket predicted to have a service life of 100 years in Example 2, FIG. (a) shows the seam opening amount Δ = 0 mm, FIG. (b) shows the seam opening amount Δ = 2 mm, and FIG. (c) shows the seam opening amount Δ = 6 mm; Fig. 9It can be seen that the stress distribution of the aged gasket under different joint opening amounts shows that as the joint opening amount decreases, the compression of the gasket increases, the holes in the gasket gradually close, and the stress concentration area at the edge of the hole increases.
[0147] The opening amount reflects the deformation of the segment joints, that is, the compression of the gasket; the greater the opening amount, the smaller the compression of the gasket, the smaller the compression force, and the smaller the contact force between the gaskets, making leakage more likely to occur.
[0148] Fig.10 It is a schematic diagram of uniaxial loading of an unaged rubber sample; in this embodiment, an unaged sealing gasket is installed in a steel mold simulating a segment groove, and a uniaxial compression test is performed using an electronic universal testing machine to obtain a compression force curve of the unaged seal.
[0149] Fig.11 is the compression force relaxation curve of the sealing gasket predicted to have a service life of 100 years in Example 2; Fig.11 It can be seen that compared with the unaged gasket, the gasket that has been in service for 100 years in the pre-compression state has a certain degree of stress relaxation, and the compression force is significantly reduced; the opening amount of the existing shield tunnel segment is usually 0-6mm, and the compression force of the gasket from the unaged to the predicted 100-year service life has decreased by 63.4% to 68.3% year-on-year;
[0150] In order to verify the accuracy of the stress relaxation model parameters, four groups of different pre-compression values Δ p =0, 2mm, 6mm, 10mm, and according to the step 1 and step 2 of the method for determining the stress relaxation model parameters of the shield tunnel aging sealing gasket of the present invention, the compressive stress-strain curves of the aging sealing gasket of the present embodiment at 4 groups of different pre-compression amounts are obtained. The aging conditions adopted in this embodiment are: the aging temperature is 75°C, and the aging time is 48h;
[0151] According to the simulation method described in Example 2, a compression force relaxation curve with a service life of 5.32 years (corresponding to the test condition: 75°C-48h) can be obtained. The comparison between the compression force relaxation test curve and the finite element software simulation result is as follows: Fig.12 ; Fig.10 Comparison results of the compression force relaxation curves of the 75℃-48h aged gaskets obtained by uniaxial compression test and finite element simulation; Fig.10 It can be seen that the simulation results of the finite element software fit well with the end points (relaxation stress) of each compression stress-strain curve, which proves that the stress relaxation model (or Mooney-Rivlin model) parameters obtained by the method described in the present invention can better reflect the stress relaxation characteristics of the sealing gasket under any pre-compression amount, and therefore can well solve the aging problem of the uneven strain distribution of the sealing gasket.
[0152] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for determining parameters of stress relaxation model of shield tunnel aging sealing gasket, characterized by: The steps include: Step 1: setting different test conditions, conducting accelerated aging tests under pre-compression on rubber samples with the same material and processing technology as the rubber sealing pad of the shield tunnel, and obtaining aged rubber samples under different test conditions; the test conditions include pre-compression strain, aging temperature and aging time; Step 2: Perform uniaxial compression tests on the unaged rubber sample and the aged rubber samples under different test conditions described in step 1 to obtain compression stress-strain curves of the unaged rubber sample and each aged rubber sample; during the uniaxial compression test, compress the aged rubber sample to the pre-compression strain before aging; Step 3: taking the ratio of the stress of the aged rubber sample at the pre-compression strain to the stress of the unaged rubber sample at the same strain as the stress relaxation coefficient, calculating the average stress relaxation coefficient of the aged rubber sample at different pre-compression strains according to the compression stress-strain curves of the unaged rubber sample and each aged rubber sample obtained in step 2, establishing an accelerated aging model with the average stress relaxation coefficient as a performance index according to the time-temperature equivalence theory and fitting to obtain a reaction constant, establishing a time-temperature conversion relationship of the aged rubber sample using the Arrhenius equation according to the reaction constant in the accelerated aging model, and converting the aging temperature and aging time of the aged rubber sample in the accelerated aging test into the service time in the actual service state according to the time-temperature conversion relationship; In step 3, the average stress relaxation coefficient of the aged rubber sample at different pre-compression strains is determined according to formula (3.1): ; In the formula, is the average stress relaxation coefficient of the aged rubber sample; K Ri is the stress relaxation coefficient of the aged rubber specimen at the i-th pre-compression strain; σ 0i is the stress of the unaged rubber specimen at the i-th pre-compression strain, σ 1i is the stress of the aged rubber specimen at the i-th pre-compression strain; i = 1, 2, ..., n, n is the number of pre-compression strains selected in the accelerated aging test; In step 3, according to the time-temperature equivalence theory, the accelerated aging model with the average stress relaxation coefficient as the performance index is established according to formula (3.2): ; Wherein, B, K, α are reaction constants; t is the rubber aging time or service time; Step 4: grouping the compression stress-strain curves of the aged rubber sample obtained in step 2 according to the service time converted in step 3, determining a compression stress-strain curve group with the same service time, interpolating any two adjacent compression stress-strain curves with different pre-compression strains in the compression stress-strain curve group according to the pre-compression strain, and obtaining a compression stress-strain curve with any pre-compression strain within the existing pre-compression strain range, and forming all compression stress-strain curves with the same service time into a compression stress-strain curve family; interpolating multiple compression stress-strain curve families with different service times of the aged rubber sample by the interpolation method; establishing a stress relaxation model based on the Mooney-Rivlin model for the aged rubber sample during the uniaxial compression test, fitting the stress relaxation model parameters corresponding to the service time according to each compression stress-strain curve family, and establishing the time-varying relationship of the model parameters under the actual service state according to the model parameters of different service times; In step 4, the interpolation method adopts the linear interpolation method; for two adjacent compression stress-strain curves of different pre-compression strains in the compression stress-strain curve group, the linear interpolation method is used to interpolate according to the pre-compression strain, and the compression stress-strain curve of any pre-compression strain within the existing pre-compression strain range is obtained as shown in formula (4.1): ; Where σ(ε) i , σ(ε) i+1 are the stresses of the aged rubber specimen at the i-th and i+1-th pre-compression strains respectively; σ(ε) i+k , ε p ,i+k , ε c ,i+k are the stress, pre-compression strain and permanent strain of the aged rubber sample at the i+kth pre-compression strain respectively; ε is the strain of the aged rubber sample in the uniaxial compression state; m is the number of interpolation between the two compression stress-strain curves of the i-th and i+1-th pre-compression strains, k is the number of the interpolation curve, k=1, 2, 3, ... m-1; where, σ(ε) i and σ(ε) i+1 , ε p ,i+k and ε c ,i+k are determined according to Equations (4.2) to (4.4): ; In the formula, ε p,i , ε p,i+1 are the i-th and i+1-th pre-compression strains set for the uniaxial compression test respectively; ε c ,i , ε c ,i+1 The permanent strains of the aged rubber specimens at the i-th and i+1-th pre-compression strains were measured in uniaxial compression tests respectively.
2. The method for determining parameters of stress relaxation model of shield tunnel aging sealing gasket according to claim 1, characterized in that: In the accelerated aging test described in step 1, the rubber sample is a cylindrical sample, the pre-compression strain range of the rubber sample is 0~ξ, ξ is the maximum pre-compression strain, ξ is -0.4~-0.6, at least 5 different pre-compression strains are set, and the interval between different pre-compression strains is less than or equal to -0.1; at least 3 different aging temperatures are set under each pre-compression strain, and the selection range of the aging temperature is 55°C~100°C; at least 5 different aging times are set under each aging temperature.
3. The method for determining parameters of stress relaxation model of shield tunnel aging sealing pad according to claim 1, characterized in that: According to the reaction constant in the accelerated aging model, the Arrhenius equation is used to establish the time-temperature conversion relationship of the aged rubber sample as shown in formula (3.3): ; Wherein, T1 is the aging temperature of the rubber sample in the accelerated aging test; T2 is the service temperature of the rubber gasket in the actual service state; t1 is the aging time of the rubber sample in the accelerated aging test; t2 is the service time of the rubber gasket in the actual service state; E is the apparent activation energy; R is the gas constant.
4. The method for determining parameters of stress relaxation model of shield tunnel aging sealing gasket according to claim 1, characterized in that: In step 4, the stress relaxation model of the rubber sample under uniaxial compression is established based on the Mooney-Rivlin model according to formula (4.5): ; Where, σ is the stress of the aged rubber sample in uniaxial compression; λ is the elongation ratio of the aged rubber sample in uniaxial compression, λ=1+ε; C 10 , C 01 are the unknown parameters of the stress relaxation model.
5. The method for determining parameters of stress relaxation model of shield tunnel aging sealing gasket according to claim 1, characterized in that: In step 4, according to the model parameters of different service times, the time-varying relationship of the model parameters under the actual service state is established according to formula (4.6): ; In the formula, m 10 , b 10 are the model parameters C 10 (t2) fitting parameters of time-varying relationship; m 01 , b 01 are the model parameters C 01 (t2) is the fitting parameter of the time-varying relationship; t2 is the service time of the rubber sealing gasket in the actual service state; C 10 (t2), C 01 (t2) is the unknown parameter of the stress relaxation model.
6. The method for determining parameters of stress relaxation model of shield tunnel aging sealing gasket according to any one of claims 1 to 5, characterized in that: When applied, the finite element software is used to establish an axial compression model of the sealing gasket, and the Mooney-Rivlin model is used in the finite element software to simulate the aged sealing gasket in the pre-compression state. According to the current service time of the aged sealing gasket in the actual service state, the corresponding stress relaxation model parameters are obtained according to the time-varying relationship of the model parameters in the actual service state. The model parameters are input into the finite element model, and the stress relaxation index of the aged sealing gasket in the pre-compression state in the actual service state is obtained after simulation and calculation. The waterproof ability of the aged sealing gasket in the current service time is determined according to the stress relaxation index; the stress relaxation index includes the compression force and average contact stress of the aged sealing gasket.