A three-phase foaming agent, alkali-activated foam concrete and preparation method thereof

By using a modified three-phase foaming agent combination in alkali-excited foam concrete, the stability of existing foaming agents in high pH environments is solved, and the high performance molding and stability of foam concrete is achieved, and the insulation is improved Performance and compressive strength reduce the risk of collapse.

CN117902850BActive Publication Date: 2024-11-08UNIV OF JINAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410081687.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-19
Publication Date
2024-11-08
Estimated Expiration
2044-01-19

AI Technical Summary

Technical Problem

The existing foaming agents have poor stability in alkali-activated foam concrete, resulting in large pores of foam concrete forming, high risk of collapse, and poor insulation performance. They show severe defoaming in high pH environments, which affects density control.

Method used

Using a combination of three-phase foaming agents, including plant protein foaming agent, xanthan gum, nanosilica, fume and sodium dodecyl sulfate, a stable gas is formed in the alkali-excited slurry by modifying the foaming agent. The liquid interface structure reduces the merger and drainage of foam, and improves the stability and pore uniformity of foam.

Benefits of technology

The foam concrete has small pores and uniform distribution in high alkaline environments, improves thermal insulation performance and compressive strength, reduces the risk of collapse, and meets the design requirements of high-performance foaming agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117902850B_ABST
    Figure CN117902850B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of foaming agents, and specifically relates to a three-phase foaming agent, alkali-activated foamed concrete and a preparation method. The present invention obtains a high-performance physical foaming agent by modifying the foaming agent, adding an appropriate amount of xanthan gum, silica fume, nano-silicon dioxide, cellulose ether and sodium dodecyl sulfate, which can adapt to a high alkaline environment, and then uses an alkali-activated gelling material as a slurry to prepare foamed concrete. The obtained foamed concrete has small foam pores and is evenly distributed, thereby improving the thermal insulation performance and strength of the foamed concrete and reducing the risk of mold collapse.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of foaming agents, and in particular relates to a three-phase foaming agent, alkali-activated foamed concrete and a preparation method thereof. Background Art

[0002] Foamed concrete has the advantages of low density, heat insulation, sound insulation, fire resistance and high temperature resistance due to the large number of pores introduced into the matrix. It is widely used in prefabricated self-insulating walls, narrow space buildings, road and bridge projects and other engineering fields. For a long time, the production of foamed concrete has used ordinary Portland Cement (OPC) as the main cementitious material, but the OPC production process is accompanied by the production of a large amount of CO2, which seriously affects the sustainable development of the ecological environment.

[0003] Alkali-activated cementitious materials are green and low-carbon cementitious materials obtained by reacting amorphous aluminum silicate solid waste materials with volcanic ash or potential hydraulic properties with alkaline activators. Compared with traditional silicate cement, alkali-activated cementitious materials not only have the characteristics of low energy consumption, high strength and good durability, but also have the characteristics of early strength and fast hardening, acid, alkali and salt corrosion resistance. It is a low-carbon green building material with great potential, and as a thermal insulation material, its fire resistance is superior to that of silicate cement-based thermal insulation materials. Therefore, combining alkali-activated materials with foam concrete to produce alkali-activated foam concrete is of great significance in promoting green buildings, energy conservation and emission reduction, and reducing energy pressure.

[0004] However, as an important component material in foamed concrete, the performance of foam will directly affect the molding of foamed concrete and the physical and chemical properties of later specimens. The stability of physical foaming agent products currently sold on the market is poor. On the one hand, after the existing commercial physical foaming agent is used in cement-based foamed concrete, it is easy to cause bubble coarsening, membrane rupture, foam drainage and other phenomena before solidification and hardening. In addition, since the alkaline environment of alkali-activated foamed concrete slurry is higher than that of cement-based materials, the stability of conventional foaming agents used for cement-based foamed concrete in alkali-activated systems will further decrease. At present, there is an urgent need for a high-performance foaming agent that can have excellent stability in a high pH environment. On the other hand, the foam produced by the foaming agent is easy to defoam during the mixing process, which makes the obtained foamed concrete molded products have large pores and easy to collapse, resulting in the performance of the foamed concrete being difficult to control, affecting engineering construction and application. In addition, the current foaming agent has serious defoaming in highly alkaline alkali-activated foamed concrete, resulting in a large difference from the designed density grade of the foamed concrete, thereby reducing its thermal insulation performance and increasing the amount of the foaming agent.

[0005] The patent application publication number CN 106588116 A discloses a nano-silica / dodecanol modified composite foaming agent and a preparation method. The composite foaming agent of the invention can be used to prepare thermal insulation cement boards, which can greatly improve the thermal insulation performance of cement boards. However, the foam stability of the foaming agent is 4-6mm in 1h, and the water secretion is 35-60ml in 1h, which has room for further optimization, and there is no description of related improvements for the performance in a high pH environment. Therefore, further improving the performance of the foaming agent and solving the application of physical foaming agents in alkali-activated foam concrete are still urgent problems to be solved. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the present invention modifies the existing commercial foaming agent to obtain a high-performance physical foaming agent that can stably exist in a highly alkaline alkali-activated slurry. The obtained foamed concrete has small pores and is evenly distributed, thereby improving the thermal insulation performance and strength of the foamed concrete and reducing its mold collapse risk.

[0007] In one aspect, the present invention provides a three-phase foaming agent, comprising the following components by mass: based on water 100%, 3%-7% of a plant protein foaming agent, 0.15%-0.25% of xanthan gum, 0.01%-0.2% of silica fume, 0.01%-0.03% of nano silicon dioxide, 0.12%-0.25% of cellulose ether, and 0.01%-0.03% of sodium lauryl sulfate. Hydroxypropyl methylcellulose and / or methylcellulose are preferred for the cellulose ether.

[0008] The present scheme is further improved, and the above-mentioned three-phase foaming agent includes the following mass components: 100% water as the base, 5% plant protein foaming agent, 0.2% xanthan gum, 0.05% silica ash, 0.025% nano silicon dioxide, 0.15% hydroxypropyl methylcellulose (HPMC), and 0.025% sodium dodecyl sulfate (SDS).

[0009] This solution is further improved, the three-phase foaming agent has a foaming multiple of 35~42 times, and the foam density is 30~40 kg / m 3 , 1h foam settling distance and 1h foam water seepage rate are both zero.

[0010] Xanthan gum and HPMC have the effect of reducing the surface tension of foam, enhancing the strength of the foam gas-liquid interface, promoting the increase of solution viscosity, and increasing the viscosity of the liquid film solution between the bubble walls of physical foam, thereby improving the adverse drainage factors caused by the movement of free water in the liquid film, and then reducing the water exudation rate of the foam.

[0011] The preferred particle size of nano-silicon dioxide is 7-40 nm and the specific surface area is 300 m 2 / g, the preferred median particle size of silica fume is 0.5 μm, and the specific surface area is 24.5 m2 / g, the particles have excellent properties such as small size and high surface free energy, can be adsorbed on the liquid / liquid and gas / liquid interfaces, increase the viscoelasticity of the liquid film, and achieve the purpose of stabilizing the foam. The nanoparticles and xanthan gum form a synergistic effect, forming a three-dimensional network structure between the foam surface and the continuous phase, preventing the aggregation and disproportionation of bubbles. In addition, nano-silica has a coagulation-promoting effect, which can quickly harden the interface between the foam and the paste in the alkali-activated foam concrete, reduce the merging and drainage of the foam, and make the prepared test block have small pores and uniform pore distribution. The addition of sodium dodecyl sulfate SDS makes the bubble size distribution more uniform, the initial foaming multiple is high, and the foam is stable.

[0012] In another aspect, the present invention provides alkali-activated foamed concrete prepared by the above three-phase foaming agent.

[0013] The present scheme is further improved, and the above-mentioned alkali-activated foamed concrete comprises the following mass components: 60%-80% slag, 20%-40% fly ash, 30%-40% sodium silicate, 4%-6% NaOH, 10%-30% water, and 6%-12% prefabricated foam, wherein the raw materials of the prefabricated foam include 100% water, 3%-7% plant protein foaming agent, 0.15%-0.25% xanthan gum, 0.01%-0.1% silica ash, 0.01%-0.03% nano-silicon dioxide, 0.12%-0.15% cellulose ether, and 0.01%-0.03% sodium dodecyl sulfate.

[0014] This scheme is further improved, alkali-activated foam concrete includes the following mass components: 70% slag, 30% fly ash, 33.64% sodium silicate, 4.22% NaOH, 16.85% water, 7.4% or 10.5% prefabricated foam, wherein the raw materials of the prefabricated foam include 100% water, 5% plant protein foaming agent, 0.2% xanthan gum, 0.05% silica ash, 0.025% nano-silicon dioxide, 0.15% hydroxypropyl methylcellulose, and 0.025% sodium lauryl sulfate.

[0015] This scheme is further improved, the slag activity index is 95%, the median particle size is 10 microns, the fly ash activity index is 75%, the median particle size is 10 microns; the activator is sodium silicate, the modulus (Na2O·3.3SiO2) is 3.3, and the solid content is 34wt%.

[0016] In a third aspect, the present invention provides a method for preparing alkali-activated foamed concrete, comprising the following steps:

[0017] (1) weighing water, vegetable protein foaming agent, xanthan gum, silica fume, nano-silicon dioxide, cellulose ether, and sodium lauryl sulfate and mixing them evenly, and passing the obtained foaming agent dilution through a foaming machine to obtain prefabricated foam for later use;

[0018] (2) First, pour the slag and fly ash into a stirring pot and stir until uniform. Then, add the activator sodium silicate, NaOH and water and stir to obtain an alkali-activated slurry.

[0019] The alkali activated slurry and an appropriate amount of the prefabricated foam obtained in step (1) are stirred and mixed evenly, poured into a mold for molding, and cured in a standard curing box to a specified age after coating.

[0020] For alkali-activated foam concrete, alkali-activated slurry can also be made of fast-hardening Portland cement, ordinary Portland cement, etc.

[0021] The present invention is further improved, and the preparation method of the above-mentioned alkali-activated foamed concrete comprises the following steps:

[0022] (1) Based on the mass percentage, 100% water is used as the basis, 5% vegetable protein, 0.2% xanthan gum, 0.05% silica fume, 0.025% nano silicon dioxide, 0.15% hydroxypropyl methylcellulose, and 0.025% sodium lauryl sulfate are mixed evenly, and the foaming agent dilution is passed through a foaming machine to obtain prefabricated foam for use;

[0023] (2) According to the mass fraction, first pour 70% blast furnace slag and 30% fly ash into a stirring pot and stir at a low speed for 60 seconds until uniform. Then slowly add 33.64% sodium silicate, 4.22% NaOH and 16.85% water and stir at a low speed for 120 seconds to obtain an alkali-activated slurry.

[0024] The alkali activated slurry and 10.5% or 7.4% of the prefabricated foam prepared in step (1) were stirred slowly for 90 seconds to mix evenly, and then quickly poured into a mold for molding. 400 kg / m 3 Or prepare 600kg / m 3 Grade foam concrete is coated and cured in a standard curing box to the specified age.

[0025] The beneficial effects of the present invention are as follows: (1) The present invention provides a solid-liquid-gas three-phase system foaming agent, modifies the existing commercial foaming agent, and adds nano-silicon dioxide and silica fume to the existing commercial plant foaming agent to enhance the gas-liquid skeleton structure on the foam surface. Nano-silicon dioxide has a coagulation-promoting effect and can rapidly harden the interface between the foam and the slurry in the alkali-activated foam concrete, thereby reducing the merging and defoaming of the foam, making the foam further stable, and making the prepared test block have small pores and uniform pore distribution. The addition of xanthan gum and HPMC reduces the water bleeding rate and sedimentation distance of the foam, and the addition of sodium dodecyl sulfate (SDS) makes the bubble size distribution more uniform. In the foaming agent synthesized by the present invention, the presence of solid particles in the foam can enhance the network structure at the air-water interface and increase the stability of the foam. Compared with the existing commercial foam foaming agent, the foam manufactured by the synthesized modified foaming agent has a longer lifespan, and avoids the phenomenon of bubble coarsening, membrane rupture, foam drainage, etc. that are easy to occur before solidification and hardening after the foaming agent is used in cement-based foam concrete. Moreover, the modified foaming agent can still foam stably in a high alkaline environment of pH=13, and the 1h foam sedimentation distance and 1h foam water seepage rate maintain the first-class foaming agent grade specified in the "JCT2199-2013 Foaming Agent" standard.

[0026] (2) The alkali-activated foamed concrete of the present invention uses alkali-activated cementitious materials as slurry, which shortens the setting and hardening time. The alkali-activated foamed concrete prepared by the alkali-activated slurry and the modified foaming agent has small pores and uniform pore distribution in the form of physical foaming, which improves the compressive strength and flexural strength of the foamed concrete, and the mold collapse phenomenon of the high-performance alkali-activated foamed concrete is greatly reduced.

[0027] (3) The modified high-performance physical foaming agent of the present invention can stably exist in a highly alkaline alkali-activated slurry, so foamed concrete of corresponding density grade can be prepared according to design requirements, thereby ensuring its thermal insulation performance and reducing the amount of foam used. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0029] Figure 1 The effect of the concentration of the foaming agent on the foam stability in Example 1;

[0030] Figure 2 The effect of the additive type on the foam stability of the foaming agent in Example 2;

[0031] Figure 3 The effect of pH value environment on foam stability of foaming agent in Example 3;

[0032] Figure 4 For the comparative example, a pure plant foaming agent was used to make 400 kg / m 3 With 600 kg / m 3 7-day and 28-day compressive and flexural strength of alkali-activated foamed concrete;

[0033] Figure 5 The modified foaming agent of Example 3 was prepared into 400 kg / m 3 With 600 kg / m 3 7-day and 28-day compressive and flexural strength of alkali-activated foamed concrete;

[0034] Figure 6 For the comparative example, a simple foaming agent was used to make 400 kg / m 3 Appearance of foamed concrete and its pore size distribution;

[0035] Figure 7 For the comparative example, a simple foaming agent was used to make 600 kg / m 3 Appearance of foamed concrete and its pore size distribution;

[0036] Figure 8 The modified foaming agent of Example 3 was made into 400kg / m 3 Appearance of foamed concrete and its pore size distribution;

[0037] Fig. 9 The modified foaming agent of Example 3 was made into 600kg / m 3 Appearance of foamed concrete and its pore size distribution.

[0038] for Figure 1 , Figure 2 , Figure 3 The lower dotted line is the benchmark control line that the 1-hour settlement distance of first-class foam should not be greater than 50mm, and the upper dotted line is the benchmark control line that the 1-hour water seepage rate of first-class foam should not be greater than 70%. DETAILED DESCRIPTION

[0039] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0040] The raw materials of alkali-activated cementitious materials: blast furnace slag (ground granulation) and fly ash (secondary) were provided by Henan Laiwu Jiuyang Steel and Shanshui Cement, respectively. The slag activity index was 95%, the median particle size was 10 microns, and the fly ash activity index was 75%, and the median particle size was 10 microns. The activator used sodium silicate with a modulus (Na2O·3.3SiO2) of 3.3 was provided by Haiwan Group, and the solid content was 34 wt%; analytical pure sodium hydroxide (NaOH) was produced by Tianjin Damao Chemical Reagent Factory.

[0041] The foaming agent used in the specific experiment is the foam concrete foaming agent produced by Sichuan Naibang Construction Co., Ltd., model NB01, which is composed of plant protein and trace animal protein. It should be noted that the animal protein component of the foaming agent used in the experiment is very small, and the main body is plant protein, which belongs to a plant protein foaming agent. The foaming agent in this experiment is the original product stock solution diluted 20 times with water as the original benchmark. It should be pointed out that the focus of the present invention is the modification of the original foaming agent, so a conventional plant protein foaming agent on the market is selected for experiment and description, which is applicable to plant protein foaming agents from different manufacturers, so the modification of different plant protein foaming agents belongs to the protection scope of the present invention.

[0042] Water: tap water refers to water that meets the relevant standards and is produced after being purified and disinfected by a water treatment plant for people's daily life and production. Domestic water is mainly obtained by pumping water from rivers, lakes, groundwater and surface water at the water plant's water intake pump station, and is obtained by the water plant in accordance with the "National Sanitary Standards for Drinking Water" through sedimentation, disinfection, filtration and other process processes.

[0043] Example 1: Selection of foaming agent

[0044] (1) The experiment used the single factor control variable method, with water as the benchmark, to change the mass fraction of different foaming agent dosages: animal protein foaming agent (Sichuan Naibang Construction Co., Ltd., model NB50, composed of bovine and sheep keratin) (3%, 5%, 7%, 10%); plant protein foaming agent (1%, 2%, 3%, 5%, 7%, 9%, 10%); the preparation method used physical foaming to prepare foam. It consists of the following steps: accurately weigh the different dosages of foaming agent and mix them evenly with water, the foaming agent dilution is passed through a foaming machine to obtain prefabricated foam, and then the foam is added to the foam stability tester to test the foam stability. The comprehensive value is (water seepage rate * sedimentation distance * 100), which is used to characterize the comprehensive stability of the foam. The smaller the value, the more stable the foam.

[0045] According to the excellent foaming agent grade specified in the "JCT2199-2013 Foaming Agent" standard, the first-class foam should have a 1-hour settlement distance of no more than 50mm and a 1-hour water seepage rate of no more than 70%; the qualified foam should have a 1-hour settlement distance of no more than 70mm and a 1-hour water seepage rate of no more than 80%. Figure 1 It can be found that the comprehensive value of animal protein foaming agent is much higher than that of plant protein foaming agent at the same concentration. When the plant protein content is 5%, the foam sedimentation distance is less than 50mm in 1h, and the water seepage rate in 1h is close to 70%. Considering the economic benefits, the plant protein foaming agent content of 5% is selected as the initial foam foaming agent content. Then the following foam stabilizer is further added to study its stability.

[0046] A vegetable protein foaming agent with a dosage of 5% was selected as the initial foaming agent dosage, and the dosage of hydroxypropyl methylcellulose (HPMC) was changed respectively (0.0025%, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%); the dosage of sodium dodecyl sulfate (SDS) was changed (0.005%, 0.025%, 0.05%, 0.1%, 0.15%); the dosage of xanthan gum was changed (0.005%, 0.025%, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%); the dosage of silica fume was changed (0.05%, 0.25%, 0.5%, 0.75%, 1%, 1.25%); the dosage of nano silicon dioxide was changed (0.0025%, 0.005%, 0.025%, 0.05%, 0.075%, 0.1%, 0.125%).

[0047] like Figure 2 As shown, the preparation method is as follows: accurately weigh the plant protein foaming agent and water and mix them evenly. Taking water as the base, first add different HPMCs with different contents and stir them evenly. The foaming agent dilution is passed through a foaming machine to obtain prefabricated modified high-performance foam, and then the foam is added to the foam stability tester to test the foam stability. Determine the lowest point of the comprehensive value, that is, the HPMC dosage is 0.15%; then take the 0.15% dosage of HPMC as the reference value, continue to add different SDS dosages, and calculate the comprehensive value of SDS, and determine the final SDS dosage to be 0.025%; based on this accumulation, the next step is to study the optimal dosage of xanthan gum, silica fume, and nano-silicon dioxide. Finally, the plant protein foaming agent dosage of 5%, HPMC 0.15%, SDS 0.025%, xanthan gum 0.2%, silica fume 0.05%, and nano-silicon dioxide 0.025% were selected as the final modified high-performance foaming agent ratio.

[0048] Example 2: Foam stability test of foaming agent

[0049] The experiment used the single-factor controlled variable method, with 100% water as the benchmark, fixed the dosage of 5% plant protein foaming agent, 0.2% xanthan gum, 0.05% silica fume, 0.025% nano-silicon dioxide, 0.15% HPMC, and 0.025% SDS, and used NaOH to adjust the pH value of the foaming agent solution (8, 9, 10, 11, 12, 13). The foaming agent dilution was passed through a foaming machine to obtain prefabricated foam, and then the foam was added to a foam stability tester to test the foam stability.

[0050] The results are as follows Figure 3 As shown, the foaming agent prepared by the present invention maintains good stability in an alkaline environment. Even when the pH value is 13, the 1-hour sedimentation distance can still be no more than 50 mm, and the 1-hour water bleeding rate can still be no more than 70%, that is, reaching the level of first-class foam.

[0051] At the same time, the pH value of the initial foam liquid prepared in this experiment is 8, and its stability has reached the requirements of the experiment. Therefore, the initial foam liquid is selected for the experiment in the next step of the experiment.

[0052] Example 3: Preparation of alkali-activated foamed concrete material

[0053] The specific preparation method consists of the following steps: taking 100% water as a base, mixing evenly with 5% vegetable protein, 0.2% xanthan gum, 0.05% silica fume, 0.025% nano silicon dioxide, 0.15% HPMC and 0.025% SDS, and passing the foaming agent dilution through a foaming machine to obtain prefabricated foam for use;

[0054] At the same time, accurately weigh 1 part of blast furnace slag and fly ash (70% slag, 30% fly ash), 33.64% sodium silicate, 4.22% NaOH, and 16.85% water. First, pour the slag and fly ash into a stirring pot, stir at a low speed for 60 seconds until uniform, then slowly add the activator (33.64% sodium silicate, 4.22% NaOH, 16.85% water) and stir at a low speed for 120 seconds to obtain an alkali-activated slurry. The alkali-activated slurry and the above-mentioned 10.5% and 7.4% prefabricated foam mass are stirred slowly for 90 seconds to mix evenly, and then quickly poured into a mold for molding to prepare 400kg / m 3 With 600kg / m 3 Grade foam concrete is coated and cured in a standard curing box to the specified age.

[0055] Comparative Example:

[0056] The specific preparation method consists of the following steps: 100% water is used as a base, mixed with 5% vegetable protein foaming agent, and the foaming agent dilution is used to obtain prefabricated foam through a foaming machine for standby use; first, 70% slag and 30% fly ash are poured into a stirring pot, stirred at a low speed for 60 seconds until uniform, and then an activator (33.64% sodium silicate, 4.22% NaOH, 16.85% water) is slowly added and stirred at a low speed for 120 seconds to obtain an alkali-activated slurry, and the above 7.4% and 10.5% prefabricated foam mass and alkali-activated slurry are respectively stirred at a slow speed for 90 seconds to mix evenly, and then quickly poured into a mold for molding to prepare 400kg / m 3 With 600kg / m 3 Grade foam concrete is coated and cured in a standard curing box to the specified age.

[0057] The specific preparation method consists of the following steps: 100% water is used as a base and mixed evenly with 3% vegetable protein foaming agent, 0.15% xanthan gum, 0.01% silica fume, 0.01% nano silicon dioxide, 0.12% hydroxypropyl methylcellulose, and 0.01% sodium lauryl sulfate, and the foaming agent dilution is passed through a foaming machine to obtain prefabricated foam for use;

[0058] At the same time, accurately weigh blast furnace slag and fly ash (60% slag, 40% fly ash), 34% sodium silicate, 4% NaOH, and 17% water. First, pour the slag and fly ash into a mixing pot, stir at a low speed for 60 seconds until uniform, then slowly add the activator (34% sodium silicate, 4% NaOH, 17% water) and stir at a low speed for 120 seconds to obtain alkali-activated slurry. The alkali-activated slurry and the above-mentioned 10.5% prefabricated foam mass are slowly stirred for 90 seconds to mix evenly, and then quickly poured into a mold to form, prepare foam concrete, and after covering, cure in a standard curing box to the specified age.

[0059] The specific preparation method comprises the following steps: 100% water is used as a base, and 7% vegetable protein, 0.25% xanthan gum, 0.2% silica fume, 0.03% nano silicon dioxide, 0.25% hydroxypropyl methylcellulose, and 0.03% sodium lauryl sulfate are uniformly mixed, and the foaming agent diluent is passed through a foaming machine to obtain prefabricated foam for use;

[0060] At the same time, accurately weigh 80% slag, 20% fly ash, 34% sodium silicate, 4% NaOH, and 17% water. First, pour the slag and fly ash into the mixing pot, stir at a low speed for 60 seconds until uniform, then slowly add the activator (34% sodium silicate, 4% NaOH, 17% water) and stir at a low speed for 120 seconds to obtain the alkali-activated slurry. The alkali-activated slurry is mixed with the above 10.5% prefabricated foam mass and stirred at a slow speed for 90 seconds, and then quickly poured into the mold to form, prepare the foamed concrete, and after covering, cure in a standard curing box to the specified age.

[0061] The difference from Example 3 is that the same mass of polyethyleneimine is used to replace HPMC.

[0062] The difference from Example 3 is that the xanthan gum is replaced by the same mass of triethanolamine.

[0063] The difference from Example 3 is that the same mass of methylcellulose is used to replace HPMC.

[0064] Through observation, for the uniformity of pore size distribution and pore size of foamed concrete, Example 3 is better than Example 8, indicating that HPMC is more suitable for the system than methyl cellulose. Example 8 is better than Example 5, and Example 5 is better than Example 4, indicating that there is a synergistic effect between the various raw materials, and a suitable ratio can play a more effective role. Example 4 is equivalent to Example 6 and Example 7, and Example 4 is better than the comparative example, indicating that the product performance can be improved by foaming agent modification, but there are very strict requirements on the selection of raw materials. The following mainly describes the performance and characteristics of Example 3 and the comparative example.

[0065] Example 7: Compression and flexural strength test of foamed concrete

[0066] The compressive and flexural strength of cement mortar after 7 days and 28 days were determined according to GB / T17671-1999 "Test Method for Strength of Cement Mortar" (ISO method). The foamed concrete specimens with the specifications of 40 mm×40 mm×160 mm were prepared in the experiment. The foamed concrete was placed in a constant temperature and humidity curing box at 20±0.5 ℃ and humidity>90% for curing to the specified age, and then the performance test was carried out. The compressive strength and flexural strength of the foamed concrete specimens cured for 7 days and 28 days were tested using a microcomputer-controlled electronic pressure testing machine. The loading speed of the electronic press was adjusted to 10 mm / min, and the pressure surface area was 40 mm×40 mm. The average value of 6 test results in each group was taken as the compressive strength value (MPa) of the specimens in that group.

[0067] The compressive and flexural strength tests were carried out using Example 3 and the comparative example. The experimental results are as follows: Figure 4 , Figure 5 As shown in the figure, it can be seen that for the concrete prepared without modified foaming agent in the comparative example, its dry density is 600kg / m 3 The concrete 7d compressive strength is 1.73MPa, the 28d compressive strength is 2.26MPa, the 7d flexural strength is 0.66MPa, and the 28d flexural strength is 0.76MPa; for the concrete prepared by the modified foaming agent in Example 3, its dry density is 600kg / m 3The concrete has a 7d compressive strength of 3.17MPa, a 28d compressive strength of 3.49MPa, a 7d flexural strength of 0.79MPa, and a 28d flexural strength of 0.92MPa. By comparison, it can be seen that after adding HPMC, SDS, xanthan gum, silica fume, and nano-silica to the original plant protein foaming agent for modification, the dry density obtained is 600kg / m 3 The compressive strength and flexural strength of foamed concrete have been significantly improved. 3 The compressive strength and flexural strength of foamed concrete have also been significantly improved.

[0068] Example 8: Foamed concrete pore size distribution

[0069] The pore size distribution of Example 3 and the comparative example was tested. Figure 6 and Figure 8 , Figure 7 and Fig. 9 As can be seen from the left figure, after adding HPMC, SDS, xanthan gum, silica fume and nano-silica to the original plant protein for modification, the pores of the foam concrete molded products become smaller and more evenly distributed, effectively reducing the risk of mold collapse.

[0070] from Figure 6 and Figure 8 , Figure 7 and Fig. 9 From the comparison of the void distribution diagram of alkali-activated foamed concrete (right figure), it can be seen that the pores larger than 800 μm in the foamed concrete made by the unmodified foaming agent are significantly more than those in the modified foamed concrete, and the number of pores smaller than 600 μm in the modified foamed concrete is also more than that in the unmodified foamed concrete. Overall, the pores in the modified foamed concrete are smaller and concentrated in the pore size range of 0-200 μm.

[0071] Although the present invention has been described in detail by referring to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention. Therefore, the scope of protection of the present invention shall be subject to the scope of protection of the claims.

Claims

1. A three-phase foaming agent, characterized in that: It includes the following mass components: based on water 100%, plant protein foaming agent 3%-7%, xanthan gum 0.15%-0.25%, silica ash 0.01%-0.2%, nano silicon dioxide 0.01%-0.03%, hydroxypropyl methylcellulose 0.12%-0.25%, sodium lauryl sulfate 0.01%-0.03%; the particle size of nano silicon dioxide is 7-40nm.

2. The three-phase foaming agent according to claim 1, characterized in that: It includes the following mass components: based on water 100%, plant protein foaming agent 5%, xanthan gum 0.2%, silica ash 0.05%, nano silicon dioxide 0.025%, hydroxypropyl methylcellulose 0.15%, and sodium lauryl sulfate 0.025%.

3. The three-phase foaming agent according to claim 1, characterized in that: The foaming multiple of the three-phase foaming agent is 35~42 times, and the foam density is 30~40 kg / m 3 , 1h foam settling distance and 1h foam water seepage rate are both zero.

4. Alkali-activated foamed concrete prepared using the three-phase foaming agent according to claim 1 or 3.

5. The alkali-activated foamed concrete according to claim 4, characterized in that: It includes the following mass components: 60%-80% slag, 20%-34% fly ash, 30%-40% sodium silicate, 4%-6% NaOH, 10%-30% water, 6%-12% prefabricated foam, wherein the raw materials of the prefabricated foam include 100% water, 3%-7% plant protein foaming agent, 0.15%-0.25% xanthan gum, 0.01%-0.1% silica ash, 0.01%-0.03% nano silicon dioxide, 0.12%-0.25% hydroxypropyl methylcellulose, and 0.1%-0.3% sodium lauryl sulfate.

6. The alkali-activated foamed concrete according to claim 5, characterized in that: It includes the following mass components: 70% slag, 30% fly ash, 33.64% sodium silicate, 4.22% NaOH, 16.85% water, 7.4% or 10.5% prefabricated foam, wherein the raw materials of the prefabricated foam include 100% water, 5% plant protein foaming agent, 0.2% xanthan gum, 0.05% silica ash, 0.025% nano silicon dioxide, 0.15% hydroxypropyl methylcellulose, and 0.025% sodium lauryl sulfate.

7. The alkali-activated foamed concrete according to claim 5, characterized in that: The activity index of slag is 95%, the median particle size is 10 microns, the activity index of fly ash is 75%, the median particle size is 10 microns; the activator is sodium silicate, the modulus is 3.3, and the solid content is 34 wt%.

8. The method for preparing alkali-activated foamed concrete according to claim 4, characterized in that: The invention comprises the following preparation methods: (1) Weighing water, vegetable protein foaming agent, xanthan gum, silica fume, nano silicon dioxide, hydroxypropyl methylcellulose, and sodium lauryl sulfate and mixing them evenly, and passing the obtained foaming agent dilution through a foaming machine to obtain prefabricated foam for later use; (2) First, pour the slag and fly ash into a mixing pot and stir until uniform, then add sodium silicate, NaOH and water and stir to obtain an alkali-activated slurry; The alkali activated slurry and an appropriate amount of the prefabricated foam obtained in step (1) are stirred and mixed evenly, poured into a mold for molding, and after coating, cured in a standard curing box to a specified age.

9. The method for preparing alkali-activated foamed concrete according to claim 8, characterized in that: The following steps are involved: (1) Based on the mass percentage, 100% water is used as the basis, 5% vegetable protein foaming agent, 0.2% xanthan gum, 0.05% silica fume, 0.025% nano silicon dioxide, 0.15% hydroxypropyl methylcellulose, and 0.025% sodium lauryl sulfate are mixed evenly, and the foaming agent dilution is passed through a foaming machine to obtain prefabricated foam for use; (2) First, pour 70% blast furnace slag and 30% fly ash into a mixing pot and stir at a low speed for 60 seconds until uniform. Then, slowly add 33.64% sodium silicate, 4.22% NaOH, and 16.85% water and stir at a low speed for 120 seconds to obtain an alkali-activated slurry. The alkali activated slurry and the 10.5% or 7.4% prefabricated foam prepared in step (1) were stirred slowly for 90 seconds to mix evenly, and then quickly poured into a mold for molding. 400 kg / m 3 or 600 kg / m 3 Grade foam concrete is coated and cured in a standard curing box to the specified age.