A graphite material and its preparation method and application

Through the combination of solvent thermal reaction and spray drying, combined with thermal curing treatment, the use of nitrogen and phosphorus inorganic salts doped with graphite materials, the problems of uniform distribution and performance stability of doped elements are solved, and the efficient electrochemical performance of lithium-ion batteries is achieved and environmentally friendly production.

CN117923483BActive Publication Date: 2024-11-08云南中晟新材料有限责任公司 +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311719021.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-14
Publication Date
2024-11-08
Estimated Expiration
2043-12-14

AI Technical Summary

Technical Problem

The prior art is difficult to achieve uniform distribution and performance stability of doped elements in graphite negative electrode materials, and the doping process cost is high, which affects the energy density and cyclic stability of lithium-ion batteries.

Method used

The method of combining solvent-thermal reaction and spray drying is adopted, combined with thermal curing treatment, and nitrogen and phosphorus inorganic salts are used as dopants to achieve uniform doping and stability improvement of graphite materials by carbonizing and graphitizing biomass.

Benefits of technology

It improves the electrochemical performance and cycle stability of graphite materials, reduces production costs, and uses waste biomass as raw materials, is environmentally friendly, and the dopants are non-toxic, achieving excellent electrochemical performance and fast charging performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004606866250000041
    Figure BDA0004606866250000041
  • Figure BDA0004606866250000051
    Figure BDA0004606866250000051
  • Figure BDA0004606866250000052
    Figure BDA0004606866250000052
Patent Text Reader

Abstract

The present invention discloses a graphite material and a preparation method and application thereof, belonging to the technical field of artificial graphite. The preparation method comprises: S1, carbonizing and graphitizing biomass to obtain a graphitized product; S2, subjecting the graphitized product prepared in step S1 to a solvent thermal reaction with ammonium polyphosphate to obtain doped graphite; S3, drying the doped graphite prepared in step S2, and performing a thermal curing treatment to obtain the graphite material. The present invention uses waste biomass as raw material, which is low-cost, renewable, and environmentally friendly, and the dopant is non-toxic, degradable, and has high production safety. At the same time, the solvent thermal reaction and the spray drying treatment are organically combined to greatly improve the uniformity of atomic doping, and combined with the thermal curing treatment, the stability and electrochemical performance of the graphite material are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of artificial graphite and relates to a graphite material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries dominate as power sources in portable electronics, have penetrated the electric vehicle market, and are about to enter the grid energy storage utility market. Graphite has good electrical conductivity and lithium ion insertion / extraction performance, making it the negative electrode material with the highest proportion and the widest commercialization in commercial lithium-ion batteries.

[0003] However, the microstructure of graphite determines that its theoretical lithium storage capacity is only 372 mAhg. -1 , which greatly restricts the energy density and cycle stability of the electrode. Element doping can significantly improve the lithium storage capacity of graphite negative electrode materials to a certain extent, and has excellent theoretical and practical research potential. However, under current conditions, the process of achieving uniform distribution of doped element atoms and compounds on graphite negative electrode materials is not mature enough, and the performance stability of negative electrode materials after doping is difficult to guarantee. Therefore, it is crucial to find simple, uniformly loaded, and effective element doping methods and processes.

[0004] Doping non-carbon elements into graphite can change the electronic state of graphite, making it easier to gain electrons, thereby further increasing Li + Int.J.Mol.Sci.2021,22,9918. Based on melamine and N 2 Pyrolysis was used as a nitrogen source to obtain nitrogen-doped starch-based carbon aerogels. The results showed that N doping had a significant effect on the electrochemical properties of potato starch carbon aerogels. An additional number of active sites were generated by doping nitrogen in the carbon structure, which further improved the lithium insertion performance. In addition, N doping promoted electronic conductivity and improved the kinetics of the electrode as well as the charge transfer transport and Li + The binding capacity of lithium ions is increased, thereby increasing the storage capacity of lithium. However, this method is cost-effective and not suitable for large-scale mass production.

[0005] Adv.Mater.Interfaces 2018,5,1701261. Nitrogen and halogen (including Cl, Br and I) dual-doped graphene was successfully synthesized by general wet chemical methods. The dual-doped heteroatoms introduced abundant defects, expanded the interlayer spacing of graphene, and facilitated the insertion and extraction of lithium. It has excellent electrochemical performance, which is mainly due to the synergistic effect of structural modification and heteroatom doping. However, the raw material CCl 4 , CBr 4 and CHI 3It is harmful to the human body, pollutes the environment, violates the principle of environmental friendliness, and cannot ensure the uniform loading of doping elements.

[0006] Therefore, how to efficiently improve the uniform loading of doping elements, ensure the stable improvement of graphite material performance, and reduce production costs remains the focus of current research. Summary of the invention

[0007] In order to solve the above technical problems, the present invention provides a graphite material and a preparation method and application thereof. The present invention organically combines solvent thermal reaction and spray drying treatment to greatly improve the uniformity of atomic doping, and combines with thermal curing treatment to effectively improve the stability and electrochemical properties of the graphite material.

[0008] In order to achieve the above object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing a graphite material, comprising the following steps:

[0010] S1, carbonizing and graphitizing the biomass to obtain a graphitized product;

[0011] S2, subjecting the graphitized product prepared in step S1 to a solvothermal reaction with ammonium polyphosphate to obtain doped graphite;

[0012] S3, drying the doped graphite prepared in step S2, and then performing a thermal curing treatment to obtain the graphite material;

[0013] The conditions of the thermal curing treatment in step S3 are: temperature 140-160° C., reaction time 1-3 h.

[0014] The drying in step S3 of the present invention is spray drying, and the water content is controlled to be no more than 2.0%.

[0015] Step S1 of the present invention has at least one of the following characteristics:

[0016] (1) The biomass is at least one of corn cobs, straw and fruit shells;

[0017] (2) The D50 of the biomass is 400-800 μm;

[0018] (3) The carbonization conditions are: carbonization temperature is 400-900° C., and carbonization time is 5-24 h;

[0019] (4) The graphitization conditions are: temperature of 2000-3000°C and time of 10-48h;

[0020] (5) The D50 of the graphitized product is 5-18 μm.

[0021] Step S2 of the present invention has at least one of the following characteristics:

[0022] (1) The conditions of the solvothermal reaction are: reaction temperature of 100-120° C., reaction time of 2-10 h, and stirring speed of 500-1000 rpm;

[0023] (2) The mass ratio of the graphitized product to ammonium polyphosphate is 1000:0.1-1000:10, and the solid content of the system in the solvent thermal reaction is 20-30%.

[0024] In some specific embodiments, the mass ratio of the graphitized product to ammonium polyphosphate is preferably 100:1-200:1.

[0025] The preparation method of the present invention also includes demagnetization and screening.

[0026] Preferably, the D50 of the graphite material after screening is 12-18 μm.

[0027] In a second aspect, the present invention provides a graphite material prepared by the preparation method.

[0028] Preferably, the graphite material of the present invention has a nitrogen content of 0.03 mass % to 0.54 mass %, and a phosphorus content of 0.04 mass % to 0.69 mass %.

[0029] In a third aspect, the present invention provides application of the graphite material in batteries.

[0030] The graphite material of the present invention can be used as a negative electrode material to prepare a negative electrode sheet of a battery.

[0031] In a fourth aspect, the present invention provides a negative electrode sheet comprising the graphite material.

[0032] Preferably, the negative electrode sheet further includes carbon black and a binder.

[0033] Fifth battery, the present invention provides a battery comprising the above-mentioned graphite material.

[0034] The beneficial effects of the present invention are:

[0035] (1) The present invention uses waste biomass as raw material, which is low-cost, renewable, and environmentally friendly, and the dopant is non-toxic, degradable, and has high production safety.

[0036] (2) The present invention uses nitrogen and phosphorus inorganic salts as dopants to achieve diatomic doping; diatomic doping produces a synergistic effect, changes the microstructure and electronic state of graphite, and expands the interlayer spacing to increase its lithium storage capacity, effectively improving the rate performance and cycle stability of graphite.

[0037] (3) During the experiment of the present invention, it was unexpectedly found that ammonium polyphosphate doping improved the hydrophilicity of the graphite surface and significantly improved its dispersibility in water, which is beneficial to the uniform dispersion of graphite in the subsequent slurry preparation process.

[0038] (4) The present invention organically combines solvent thermal reaction and spray drying treatment, greatly improving the uniformity of atomic doping, achieving uniform loading of heteroatoms, and combining with thermal curing treatment, effectively improving the stability and electrochemical properties of graphite materials.

[0039] (5) The lithium-ion battery assembled with the graphite material prepared by the present invention has excellent electrochemical properties. After 300 cycles, the capacity retention rate is ≥96%, and can reach up to 97.12%, and has excellent fast charging performance. DETAILED DESCRIPTION

[0040] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0041] Before further describing the specific embodiments of the present invention, it should be understood that the scope of protection of the present invention is not limited to the specific embodiments described below; it should also be understood that the terms used in the examples of the present invention are for describing specific embodiments rather than for limiting the scope of protection of the present invention.

[0042] When the embodiment gives a numerical range, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the present invention belongs.

[0043] The present invention does not limit the sources of the raw materials used. Unless otherwise specified, the raw materials used in the present invention are common commercial products in the technical field.

[0044] Examples 1-4 and Comparative Examples 1-2

[0045] Preparation method: The graphite material is prepared according to the process parameters in Table 1, specifically:

[0046] (1) taking a biomass raw material, crushing it, controlling the D50 to be 400-800 μm, drying it, placing the dried biomass particles in a carbonization furnace, and carbonizing them under a nitrogen atmosphere at a heating rate of 2-5° C. / min, a carbonization temperature of 400-900° C., and a carbonization time of 5-24 h to obtain biochar;

[0047] (2) graphitizing the biochar in an inert gas atmosphere at a temperature of 2000-3000° C. for 10-48 h to obtain a graphitized product with a D50 of 5-18 μm;

[0048] (3) mixing the graphitized product, nitrogen and phosphorus inorganic salts and water in a certain proportion for solvothermal reaction at a reaction temperature of 100-120° C., a reaction time of 2-10 h, and a rotation speed of 500-1000 rpm to obtain doped graphite;

[0049] (4) After the doped graphite is spray-dried, it is heat-cured at 140-160° C. for 1-3 h, electrically impurities are removed for 3 times, and sieved to obtain a graphite material with a D50 of 12-18 μm.

[0050] Table 1 Process parameters of Examples 1-4 and Comparative Examples 1-2

[0051]

[0052]

[0053] Among them, # indicates that the biomass is corn cob, ▲ indicates that the biomass is straw, and Δ indicates that the biomass is fruit shell.

[0054] Test Example 1

[0055] The products prepared in Example 1-4 and Comparative Example 1-2 were dispersed in water (temperature was 25° C.), and other conditions were kept the same. The time required for them to be uniformly dispersed in water was compared. The results are shown in Table 2.

[0056] The experiment found that compared with other inorganic phosphates, ammonium polyphosphate doping improves the hydrophilicity of the graphite surface and significantly improves its dispersibility in water, which is beneficial to the uniform dispersion of graphite in the subsequent slurry preparation process.

[0057] Table 2 Hydrophilic properties of graphite materials

[0058]

[0059]

[0060] Example 1 and Comparative Examples 3-6

[0061] Preparation method: As in the above-mentioned Example 1, the graphite material is prepared specifically according to the process parameters in Table 3.

[0062] Table 3 Process parameters of comparative examples 3-6

[0063]

[0064]

[0065] Among them, # indicates that the biomass is corn cob, ▽ represents oven vacuum drying, ◇ represents ball milling, and the ball milling time is 5 h.

[0066] Application Example 2

[0067] The graphite materials obtained in Examples 1-4 and Comparative Examples 1-5 were used as negative electrodes and mixed with conductive carbon black (Surper P) and PAA binder in a mass ratio of 96.5:1.5:2.0 to obtain slurry, which was then coated on copper foil to form a negative electrode sheet.

[0068] The prepared negative electrode plate and the lithium metal plate were assembled into a lithium-ion button cell, and LiPF6 was dissolved in an electrolyte of ethylene carbonate / diethyl carbonate / ethyl methyl carbonate = 2:3:1 at a concentration of 1 mol / L. After the button cell assembly was completed, cycle and rate performance tests were carried out.

[0069] The results are shown in Table 4.

[0070] Comparing Example 1 with Comparative Examples 1-2, the samples prepared in Comparative Examples 1 and 2 using conventional nitrogen and phosphorus inorganic salts as dopants can also achieve doping of nitrogen and phosphorus diatoms at the same time, but compared with Example 1 using ammonium polyphosphate as a dopant, their cycle stability and rate performance are significantly deteriorated. This may be because ammonium polyphosphate doping improves the hydrophilicity of the graphite surface and makes the graphite more evenly dispersed in the slurry.

[0071] Compared with Example 1 and Comparative Example 5, the spray drying method has better rate performance and cycle stability than the samples prepared by other drying methods. This may be because spray drying is a method of atomizing a solution or suspension into small droplets through a spray head and then drying it quickly in a hot air flow. This method can produce uniform particles and can evenly disperse the active ingredients in the carrier, which is conducive to uniform loading of the elements.

[0072] Comparing Example 1 with Comparative Examples 3-4, the changes in moisture content and thermal curing temperature after spray drying have a certain influence on the rate performance and cycle stability of the prepared samples.

[0073] Comparing Example 1 with Comparative Example 6, the solvothermal method is more conducive to heteroatom doping, and the ball milling method may destroy the layered structure of graphite, thereby affecting its performance.

[0074] Table 4 Electrochemical properties of graphite materials

[0075]

[0076]

[0077] The above is a further description of the present invention in conjunction with specific embodiments, but these embodiments are merely exemplary and do not constitute any limitation on the scope of the present invention. It should be understood by those skilled in the art that the details and forms of the technical solution of the present invention may be modified or replaced without departing from the spirit and scope of the present invention, but these modifications and replacements all fall within the scope of protection of the present invention.

Claims

1. A method for preparing a graphite material, characterized in that: The steps include: S1, carbonizing and graphitizing the biomass to obtain a graphitized product; S2, subjecting the graphitized product prepared in step S1 to a solvothermal reaction with ammonium polyphosphate to obtain doped graphite; S3, drying the doped graphite prepared in step S2, and performing a thermal curing treatment to obtain the graphite material; the moisture content after drying is controlled to be no more than 2.0%; The conditions of the thermal curing treatment are: temperature 140-160° C., reaction time 1-3 hours.

2. The preparation method according to claim 1, characterized in that: Step S1 has at least one of the following characteristics: (1) The biomass is at least one of corn cobs, straw and fruit shells; (2) The D50 of the biomass is 400-800 μm; (3) The carbonization conditions are: carbonization temperature is 400-900° C., and carbonization time is 5-24 h; (4) The graphitization conditions are: temperature of 2000-3000°C and time of 10-48h; (5) The D50 of the graphitized product is 5-18 μm.

3. The preparation method according to claim 1, characterized in that: Step S2 has at least one of the following characteristics: (1) The conditions of the solvothermal reaction are: reaction temperature of 100-120° C., reaction time of 2-10 h, and stirring speed of 500-1000 rpm; (2) The mass ratio of the graphitized product to ammonium polyphosphate is 1000:0.1-1000:10, and the solid content of the system in the solvent thermal reaction is 20-30%.

4. The graphite material prepared by the preparation method according to any one of claims 1 to 3.

5. The graphite material according to claim 4, characterized in that The graphite material contains nitrogen at a content of 0.03 mass % to 0.54 mass %, and phosphorus at a content of 0.04 mass % to 0.69 mass %.

6. Use of the graphite material according to any one of claims 4 or 5 in batteries.

7. A negative electrode sheet, characterized in that: The invention comprises the graphite material as described in any one of claims 4 to 6.