A high-efficiency flame retardant of chlorinated paraffin composite montmorillonite and its application

By modifying montmorillonite with chlorinated paraffin-based quaternary ammonium salt intercalation, the problem of the influence of flame retardants on the mechanical properties of plastic products and the insufficient heat resistance of chlorinated paraffin was solved, and efficient flame retardancy and mechanical properties were achieved. Improved, forming a highly efficient chlorinated paraffin composite montmorillonite flame retardant.

CN117924950BActive Publication Date: 2024-10-01ANHUI XINGXIN MATERIAL TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202311646712.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-04
Publication Date
2024-10-01
Estimated Expiration
2043-12-04

AI Technical Summary

Technical Problem

While existing flame retardants improve the flame retardant properties of plastic products, they often affect their mechanical properties, and chlorinated paraffins have insufficient heat resistance, making it difficult to be widely used in flame retardant plastics.

Method used

Chlorinated paraffin-based quaternary ammonium salts are used to intercalate and modify montmorillonite to increase its interlayer spacing and surface activity, improve dispersion with the polymer matrix, and absorb flammable gases and heat insulation effects through the hole structure of montmorillonite. , synergistically exerting flame retardant effect.

Benefits of technology

The synergistic effect of high flame retardancy and high mechanical properties is achieved at low addition amounts, which improves the heat resistance and flame retardancy of plastic products and avoids the problem of melting and dripping of chlorinated paraffin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117924950B_ABST
    Figure CN117924950B_ABST
Patent Text Reader

Abstract

The present invention provides a high-efficiency flame retardant of chlorinated paraffin composite montmorillonite and its application. The high-efficiency flame retardant of chlorinated paraffin composite montmorillonite is obtained by subjecting montmorillonite to intercalation modification reaction with chlorinated paraffin-based quaternary ammonium salt. The high-efficiency flame retardant of chlorinated paraffin composite montmorillonite and its application provided by the present invention adopts chlorinated paraffin composite montmorillonite as a high-efficiency flame retardant to flame retardant modification of plastic products, so that halogen flame retardant chlorinated paraffin and inorganic flame retardant montmorillonite can play a synergistic role, and high flame retardancy and high mechanical properties of polymer plastic products can be achieved under the premise of low addition amount.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of flame retardant materials, in particular to a high-efficiency flame retardant of chlorinated paraffin composite montmorillonite and application thereof. Background Art

[0002] People's use and application of plastic polymer materials are rapidly increasing, and in daily life, the application field of plastic products is becoming more and more extensive. However, once a fire occurs in plastic products as polymer materials, the consequences are very serious. A large amount of toxic and harmful gases are produced during the combustion process, which poses an extremely huge threat to humans and the surrounding environment. This puts forward corresponding high requirements for the flame retardant properties of plastic products. Today, the research on flame retardancy of plastic products has been very extensive and in-depth. Strict flame retardant standards and environmental protection regulations have been gradually implemented and applied to all aspects of modern life. High-efficiency, low-smoke, low-toxic, green and environmentally friendly flame retardants have become the development trend of flame retardants.

[0003] At present, the flame retardant modification of plastic products is mainly achieved by adding flame retardants. However, most of the added flame retardants have a negative impact on the mechanical and processing properties of plastic products, and some of the impacts are even very serious. Therefore, how to solve the contradiction between high flame retardancy and mechanical properties has become a difficult problem for high-quality flame retardant plastic products.

[0004] Chlorine-based flame retardants are commonly used flame retardant additives for plastic products. They mainly achieve flame retardancy through the gas phase flame retardant mechanism. Not only can they inhibit the combustion chain reaction, but their pyrolysis products can also be used as inert substances to dilute the concentration of combustible gases. As halogen-containing compounds, the flame retardant mode of chlorine-based flame retardants is to release halogen and hydrogen halide at high temperatures, among which hydrogen halide can capture highly active free radicals H·, O· and OH·, while generating halogen free radicals with lower energy, and finally terminate the chain combustion reaction. However, due to the insufficient flame retardant efficiency or heat resistance of chlorine-based flame retardants (such as chlorinated paraffin), they cannot be widely used in flame-retardant plastic products.

[0005] Montmorillonite is a layered chain inorganic nanomaterial. In the prior art, it is effectively compounded with plastic polymer materials to form composite plastic products with excellent mechanical, flame retardant and other properties. The reason why this composite plastic product shows its excellent performance compared with traditional composite plastic products is that there is a strong interaction between the polymer matrix and the organic montmorillonite. On the one hand, since the macromolecular chains of the polymer are confined in the middle layer of the montmorillonite, the movement of the macromolecular chains is hindered. In addition, the particle size of the organic montmorillonite is small, its surface area is large, and there are many surface active centers. It can be closely combined with the polymer matrix and has good compatibility, thus showing excellent mechanical properties; on the other hand, since montmorillonite itself is non-flammable, when the polymer macromolecular chains are confined in the interlayer of montmorillonite, the movement of the macromolecules is restricted, which hinders the formation of volatile gases during the combustion process.

[0006] However, the premise of using montmorillonite to form composite plastic products with excellent mechanical, flame retardant and other properties is that the montmorillonite can be effectively dispersed when added to the polymer matrix. At present, if the montmorillonite is not modified, there will be a problem of poor dispersion when the montmorillonite is added to the polymer matrix. At this time, only a small amount of montmorillonite can be added to the matrix to avoid the agglomeration of montmorillonite and affect the physical and mechanical properties of the composite material. However, it is difficult to achieve the ideal modification effect with a small amount of montmorillonite. Summary of the invention

[0007] Based on the technical problems existing in the background technology, the present invention proposes a high-efficiency flame retardant of chlorinated paraffin composite montmorillonite and its application, and adopts chlorinated paraffin composite montmorillonite as a high-efficiency flame retardant to perform flame retardant modification on plastic products, so that the halogen flame retardant chlorinated paraffin and the inorganic flame retardant montmorillonite can play a synergistic role, and high flame retardancy and high mechanical properties of polymer plastic products can be achieved under the premise of low addition amount.

[0008] The invention provides a high-efficiency flame retardant of chlorinated paraffin composite montmorillonite, which is obtained by subjecting montmorillonite to an intercalation modification reaction with a chlorinated paraffin-based quaternary ammonium salt.

[0009] In the present invention, montmorillonite is intercalated and modified by using chlorinated paraffin-based quaternary ammonium salt. On the one hand, the chlorinated paraffin-based quaternary ammonium salt increases the interlayer distance of the inorganic montmorillonite, improves the expansion performance, and brings organic components into the interlayer, thereby improving the interface polarity and chemical microenvironment of the inorganic matter, and finally improving the dispersibility of the montmorillonite and the chlorinated paraffin intercalated therein in the polymer matrix, which not only reduces the mobility of small molecules of flame retardants such as chlorinated paraffin, so that the montmorillonite and the chlorinated paraffin can better play a synergistic effect, but also is conducive to the effective dispersion of the montmorillonite in the polymer matrix, thereby obtaining excellent mechanical improvement performance; on the other hand, the pore structure of the montmorillonite in the obtained high-efficiency flame retardant can absorb a large amount of combustible gas, delay the escape of volatile products generated during the thermal decomposition of the polymer material, and help to exert the flame retardant effect, and the heat insulation effect of the montmorillonite itself can avoid the defect that the chlorinated paraffin alone is easily melted and dripped when added to the polymer, and objectively overcomes the defect of insufficient heat resistance.

[0010] Preferably, the chlorinated paraffin-based quaternary ammonium salt is obtained by subjecting chlorinated paraffin to a nucleophilic substitution reaction with a tertiary amine compound.

[0011] Preferably, the tertiary amine compound is a tertiary amine compound containing alkoxysilane;

[0012] Preferably, the tertiary amine compound containing alkoxysilane is obtained by subjecting a silane coupling agent containing an epoxy group to a ring-opening reaction with N,N-dimethylethanolamine;

[0013] Preferably, the epoxy group-containing silane coupling agent is at least one of γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane or β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, preferably γ-glycidyloxypropyltrimethoxysilane.

[0014] In the present invention, when the silane coupling agent containing an epoxy group is γ-glycidyloxypropyltrimethoxysilane, the structure of the tertiary amine compound containing an alkoxysilane is as follows:

[0015]

[0016] In the present invention, chlorinated paraffin and a tertiary amine compound containing alkoxysilane are selected to undergo a nucleophilic substitution reaction, and the structure of the obtained chlorinated paraffin-based quaternary amine contains an alkoxysilane group. In addition to being able to perform intercalation modification on montmorillonite, the alkoxysilane can also condense with the hydroxyl group on the montmorillonite, which cannot further increase the surface lipophilicity of the montmorillonite, is beneficial to the dispersion of the montmorillonite in the polymer matrix, and also improves the anchoring property of the chlorinated paraffin in the montmorillonite to avoid migration, thereby effectively exerting a flame retardant effect.

[0017] Preferably, the mass ratio of the chlorinated paraffin to the tertiary amine compound is 1:1-3;

[0018] Preferably, the temperature of the nucleophilic substitution reaction is 70-90° C. and the time is 1-3 h.

[0019] Preferably, the montmorillonite is at least one of sodium-based montmorillonite, calcium-based montmorillonite and magnesium-based montmorillonite.

[0020] Preferably, the mass ratio of the chlorinated paraffin-based quaternary ammonium salt to montmorillonite is 1:3-5.

[0021] Preferably, the temperature of the intercalation modification reaction is 80-100° C. and the time is 4-8 hours.

[0022] The present invention also provides a method for preparing the above-mentioned chlorinated paraffin composite montmorillonite high-efficiency flame retardant, comprising:

[0023] (1) mixing chlorinated paraffin and a tertiary amine compound, heating to 70-90° C. and stirring for reaction for 1-3 hours to obtain a chlorinated paraffin-based quaternary ammonium salt;

[0024] (2) After montmorillonite is dispersed evenly with a dispersion medium, the chlorinated paraffin-based quaternary ammonium salt is added and mixed evenly, the temperature is raised to 80-100° C. and stirred for reaction for 4-8 hours, filtered, washed, and dried to obtain the chlorinated paraffin-composite montmorillonite high-efficiency flame retardant.

[0025] Preferably, the dispersion medium is at least one of water, ethanol or methanol, and the content of the montmorillonite after being evenly dispersed in the dispersion medium is 1-5 wt%.

[0026] The present invention also proposes the use of the chlorinated paraffin composite montmorillonite high-efficiency flame retardant in flame-retardant plastics.

[0027] Preferably, the flame retardant plastic comprises a polymer matrix and the high-efficiency flame retardant;

[0028] Preferably, the polymer matrix is ​​at least one of PE, PP, PA, PC, PBT or ABS;

[0029] Preferably, the amount of the high-efficiency flame retardant is 1-20 wt % of the polymer matrix.

[0030] In the present invention, in the high-efficiency flame retardant of the chlorinated paraffin composite montmorillonite, the montmorillonite is intercalated and modified by using the chlorinated paraffin-based quaternary ammonium salt, so that the organic components are introduced into the interlayer of the montmorillonite, and the lipophilicity thereof is improved. With the increase of the lipophilicity of the montmorillonite, the interaction force between the montmorillonite and the polymer matrix is ​​enhanced, resulting in an increase in the viscosity of the system, a decrease in the fluidity of the polymer matrix, and difficulty in forming dripping. In addition, after being heated, the chlorinated paraffin generates an unstable free Cl structure and captures the H free radicals in the polymer matrix. Although the formed HCl gas can play a flame retardant effect, the HCl gas is corrosive to the environment. Considering that the intercalation structure of the montmorillonite can effectively adsorb the HCl gas so that it does not diffuse into the environment, the high-efficiency flame retardant of the present invention is also beneficial to the environment. Furthermore, after the polymer material is strongly heated, the montmorillonite can form multiple layers of black flocculent carbon-containing aluminum silicate residues on the surface of the polymer, which migrate to the surface of the material to form a protective layer, thereby improving the thermal stability of the polymer and helping the chlorinated paraffin to play a flame retardant effect in plastic products.

[0031] In the present invention, compared with simply physically blending chlorinated paraffin and montmorillonite as a flame retardant, montmorillonite is intercalated and modified with chlorinated paraffin-based quaternary ammonium salt as a flame retardant. The latter can significantly reduce the amount of flame retardant without reducing the flame retardant level. It can be seen that chlorinated paraffin and montmorillonite have a certain synergistic flame retardant effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The infrared spectra of montmorillonite before and after being modified by the chlorinated paraffin-based quaternary ammonium salt intercalation described in Example 1;

[0033] Figure 2 The thermogravimetric analysis diagrams of the flame retardants described in Example 1 and Comparative Examples 1 and 2 are shown. DETAILED DESCRIPTION

[0034] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.

[0035] Example 1

[0036] This embodiment provides a high-efficiency flame retardant of chlorinated paraffin composite montmorillonite, which is prepared by the following method:

[0037] (1) N,N-dimethylethanolamine mixed with tin tetrachloride (catalyst) is added dropwise to γ-glycidyloxypropyltrimethoxysilane, wherein the mass ratio of tin tetrachloride, N,N-dimethylethanolamine, and γ-glycidyloxypropyltrimethoxysilane is 0.01:1:2.8. After the addition is completed, the temperature is raised to 60° C. and stirred for a ring-opening reaction for 3 hours to obtain a tertiary amine compound containing an alkoxysilane;

[0038] (2) mixing chlorinated paraffin and the above-mentioned alkoxysilane-containing tertiary amine compound in a mass ratio of 1:2, heating to 80° C. and stirring for 2 h to obtain a chlorinated paraffin-based quaternary ammonium salt;

[0039] (3) Dispersing sodium-based nano-montmorillonite (particle size of 60 nm) in water and stirring to disperse evenly to obtain a nano-montmorillonite dispersion with a concentration of 3 wt%, adding the above-mentioned chlorinated paraffin-based quaternary ammonium salt to the nano-montmorillonite dispersion, the mass ratio of the chlorinated paraffin-based quaternary ammonium salt to the sodium-based nano-montmorillonite being 1:4, stirring and mixing evenly, heating to 90° C. and stirring to react for 6 h, filtering, washing with water, and drying the filter cake to obtain the high-efficiency flame retardant of the chlorinated paraffin-based composite montmorillonite.

[0040] This embodiment also proposes a flame-retardant plastic, which is obtained by adding the above-mentioned high-efficiency flame retardant of chlorinated paraffin composite montmorillonite and polypropylene into a high-speed mixer and blending them evenly, wherein the amount of the high-efficiency flame retardant of chlorinated paraffin composite montmorillonite is 5wt% of the polypropylene, and then adding the obtained blended material into a twin-screw extruder, extruding and granulating in the temperature range of 165-195°C, and melt injection molding at 250°C to obtain the flame-retardant plastic.

[0041] The montmorillonite before and after the modification by the chlorinated paraffin-based quaternary ammonium salt intercalation described in Example 1 was tested by infrared absorption spectrum. The results are shown in Table 1. Figure 1 , Figure 1 The infrared spectra of montmorillonite before and after modification by chlorinated paraffin-based quaternary ammonium salt intercalation described in Example 1 are shown in FIG. Figure 1 It can be seen that the montmorillonite modified by the chlorinated paraffin-based quaternary ammonium salt intercalation described in Example 1 has a carbon content of 763 cm -1 The absorption peak at 1288 cm -1 The absorption peak at 1732 cm -1 and 2018cm -1 The absorption peak at is the characteristic absorption peak of C-Cl.

[0042] Example 2

[0043] This embodiment provides a high-efficiency flame retardant of chlorinated paraffin composite montmorillonite, which is prepared by the following method:

[0044] (1) adding N,N-dimethylethanolamine mixed with tin tetrachloride (catalyst) dropwise to γ-glycidyloxypropyltriethoxysilane, wherein the mass ratio of tin tetrachloride, N,N-dimethylethanolamine and γ-glycidyloxypropyltriethoxysilane is 0.01:1:3. After the addition is completed, the temperature is raised to 60° C. and stirred for a ring-opening reaction for 3 hours to obtain a tertiary amine compound containing an alkoxysilane;

[0045] (2) mixing chlorinated paraffin and the above-mentioned alkoxysilane-containing tertiary amine compound in a mass ratio of 1:3, heating to 70° C. and stirring for reaction for 3 hours to obtain a chlorinated paraffin-based quaternary ammonium salt;

[0046] (3) Dispersing sodium-based nano-montmorillonite (particle size of 60 nm) in water and stirring to disperse evenly to obtain a nano-montmorillonite dispersion with a concentration of 1 wt%, adding the above-mentioned chlorinated paraffin-based quaternary ammonium salt to the nano-montmorillonite dispersion, the mass ratio of the chlorinated paraffin-based quaternary ammonium salt to the sodium-based nano-montmorillonite being 1:5, stirring and mixing evenly, heating to 80° C. and stirring to react for 8 h, filtering, washing with water, and drying the filter cake to obtain the high-efficiency flame retardant of the chlorinated paraffin-based composite montmorillonite.

[0047] This embodiment also proposes a flame-retardant plastic, which is obtained by adding the above-mentioned high-efficiency flame retardant of chlorinated paraffin composite montmorillonite and polypropylene into a high-speed mixer and blending them evenly, wherein the amount of the high-efficiency flame retardant of chlorinated paraffin composite montmorillonite is 5wt% of the polypropylene, and then adding the obtained blended material into a twin-screw extruder, extruding and granulating in the temperature range of 165-195°C, and melt injection molding at 250°C to obtain the flame-retardant plastic.

[0048] Example 3

[0049] This embodiment provides a high-efficiency flame retardant of chlorinated paraffin composite montmorillonite, which is prepared by the following method:

[0050] (1) N,N-dimethylethanolamine mixed with tin tetrachloride (catalyst) is added dropwise to β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, wherein the mass ratio of tin tetrachloride, N,N-dimethylethanolamine, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane is 0.01:1:3. After the addition is completed, the temperature is raised to 60° C. and stirred for a ring-opening reaction for 3 hours to obtain a tertiary amine compound containing an alkoxysilane;

[0051] (2) mixing chlorinated paraffin and the above-mentioned alkoxysilane-containing tertiary amine compound in a mass ratio of 1:1, heating to 90° C. and stirring for 1 hour to obtain a chlorinated paraffin-based quaternary ammonium salt;

[0052] (3) Dispersing sodium-based nano-montmorillonite (particle size of 60 nm) in water and stirring to disperse evenly to obtain a nano-montmorillonite dispersion with a concentration of 5 wt%, adding the above-mentioned chlorinated paraffin-based quaternary ammonium salt to the nano-montmorillonite dispersion, the mass ratio of the chlorinated paraffin-based quaternary ammonium salt to the sodium-based nano-montmorillonite being 1:3, stirring and mixing evenly, heating to 100° C. and stirring to react for 4 hours, filtering, washing with water, and drying the filter cake to obtain the high-efficiency flame retardant of the chlorinated paraffin composite montmorillonite.

[0053] This embodiment also proposes a flame-retardant plastic, which is obtained by adding the above-mentioned high-efficiency flame retardant of chlorinated paraffin composite montmorillonite and polypropylene into a high-speed mixer and blending them evenly, wherein the amount of the high-efficiency flame retardant of chlorinated paraffin composite montmorillonite is 5wt% of the polypropylene, and then adding the obtained blended material into a twin-screw extruder, extruding and granulating in the temperature range of 165-195°C, and melt injection molding at 250°C to obtain the flame-retardant plastic.

[0054] Comparative Example 1

[0055] This comparative example proposes a flame retardant, which is prepared by the following method:

[0056] Sodium-based nano-montmorillonite (with a particle size of 60 nm) is dispersed in water and stirred to be uniformly dispersed to obtain a nano-montmorillonite dispersion with a concentration of 3wt%, and chlorinated paraffin is added to the nano-montmorillonite dispersion, wherein the mass ratio of the chlorinated paraffin to the sodium-based nano-montmorillonite is 1:4. After stirring and mixing evenly, the mixture is heated to 90°C and stirred for reaction for 6 hours, filtered, washed with water, and the filter cake is dried to obtain the flame retardant.

[0057] This comparative example also proposes a flame-retardant plastic, which is obtained by adding the above-mentioned flame retardant and polypropylene into a high-speed mixer and blending them evenly, wherein the amount of the flame retardant is 5wt% of the polypropylene, and then adding the obtained blended material into a twin-screw extruder, extruding and granulating in the temperature range of 165-195°C, and melt injection molding at 250°C to obtain the flame-retardant plastic.

[0058] Comparative Example 2

[0059] This comparative example proposes a flame retardant, which is prepared by the following method:

[0060] (1) mixing chlorinated paraffin and N,N-dimethylethanolamine in a mass ratio of 1:2, heating to 80° C. and stirring for 2 h to obtain a quaternary ammonium salt of chlorinated paraffin;

[0061] (2) Dispersing sodium-based nano-montmorillonite (particle size of 60 nm) in water and stirring to disperse evenly to obtain a nano-montmorillonite dispersion with a concentration of 3 wt%, adding the above-mentioned chlorinated paraffin-based quaternary ammonium salt to the nano-montmorillonite dispersion, wherein the mass ratio of the chlorinated paraffin-based quaternary ammonium salt to the sodium-based nano-montmorillonite is 1:4, stirring and mixing evenly, heating to 90° C. and stirring to react for 6 h, filtering, washing with water, and drying the filter cake to obtain the flame retardant.

[0062] This comparative example also proposes a flame-retardant plastic, which is obtained by adding the above-mentioned high-efficiency flame retardant of chlorinated paraffin composite montmorillonite and polypropylene into a high-speed mixer and blending them evenly, wherein the amount of the high-efficiency flame retardant of chlorinated paraffin composite montmorillonite is 5wt% of the polypropylene. The obtained blended material is then added into a twin-screw extruder, extruded and granulated in the temperature range of 165-195°C, and melt injection molded at 250°C to obtain the flame-retardant plastic.

[0063] The flame retardants described in Example 1 and Comparative Examples 1 and 2 were subjected to TGA test. The results are as follows: Figure 2 As shown, Figure 2 The thermogravimetric analysis diagram of the flame retardant described in Example 1 and Comparative Examples 1 and 2 is shown in FIG. Figure 2 It can be seen that, compared with the flame retardants described in Comparative Examples 1 and 2, it can be clearly seen that the thermal decomposition temperature of the flame retardant described in Example 1 is significantly increased, and the heat resistance is enhanced.

[0064] According to the ASTM D2863-70 standard, the flame retardant plastics described in the embodiments and comparative examples were tested for limiting oxygen index (LOI) using an oxygen index tester, and the flame retardant plastics described in the embodiments and comparative examples were tested for horizontal vertical combustion (UL-94) using a horizontal vertical combustion analyzer;

[0065] The mechanical properties of the flame retardant plastics described in the embodiments and comparative examples were tested with reference to GB / T 1040-2018, GB / T 21189-2007 and GB / T 9341-2008 standards;

[0066] The results are shown in Table 1 below:

[0067] Table 1 Performance test results of the flame retardant plastics described in the embodiments and comparative examples

[0068]

[0069] It can be seen from Table 1 above that although the simple addition of montmorillonite and chlorinated paraffin has a certain flame retardant effect, the effect is not ideal, and there is a melt dripping phenomenon; and, compared with the common chlorinated paraffin-based quaternary ammonium salt intercalation modified montmorillonite, after the chlorinated paraffin-based quaternary ammonium salt intercalation modified montmorillonite of the present invention is used, the interlayer spacing of the montmorillonite and the thermal stability of the montmorillonite are greatly improved, and the flame retardant and mechanical properties are also greatly improved.

[0070] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high-efficiency flame retardant of chlorinated paraffin composite montmorillonite, characterized in that: It is obtained by intercalating montmorillonite with chlorinated paraffin-based quaternary ammonium salt; The chlorinated paraffin-based quaternary ammonium salt is obtained by subjecting chlorinated paraffin to a nucleophilic substitution reaction with a tertiary amine compound; the tertiary amine compound is a tertiary amine compound containing alkoxysilane.

2. The high-efficiency flame retardant of chlorinated paraffin composite montmorillonite according to claim 1, characterized in that: The tertiary amine compound containing alkoxysilane is obtained by subjecting a silane coupling agent containing an epoxy group to a ring-opening reaction with N,N-dimethylethanolamine.

3. The high-efficiency flame retardant of chlorinated paraffin composite montmorillonite according to claim 2, characterized in that: The epoxy group-containing silane coupling agent is at least one of γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane or β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.

4. The high-efficiency flame retardant of chlorinated paraffin composite montmorillonite according to any one of claims 1 to 3, characterized in that: The mass ratio of the chlorinated paraffin to the tertiary amine compound is 1:1-3.

5. The high-efficiency flame retardant of chlorinated paraffin composite montmorillonite according to any one of claims 1 to 3, characterized in that: The temperature of the nucleophilic substitution reaction is 70-90° C. and the time is 1-3 h.

6. The high-efficiency flame retardant of chlorinated paraffin composite montmorillonite according to any one of claims 1 to 3, characterized in that: The montmorillonite is at least one of sodium-based montmorillonite, calcium-based montmorillonite and magnesium-based montmorillonite.

7. The high-efficiency flame retardant of chlorinated paraffin composite montmorillonite according to any one of claims 1 to 3, characterized in that: The mass ratio of the chlorinated paraffin-based quaternary ammonium salt to montmorillonite is 1:3-5.

8. The high-efficiency flame retardant of chlorinated paraffin composite montmorillonite according to any one of claims 1 to 3, characterized in that: The temperature of the intercalation modification reaction is 80-100° C. and the time is 4-8 hours.

9. A method for preparing a high-efficiency flame retardant of chlorinated paraffin composite montmorillonite according to any one of claims 1 to 8, characterized in that: include: (1) After mixing chlorinated paraffin and tertiary amine compounds, heating to 70-90°C and stirring for reaction for 1-3 hours to obtain chlorinated paraffin-based quaternary ammonium salt; (2) After the montmorillonite is dispersed evenly with a dispersion medium, the chlorinated paraffin-based quaternary ammonium salt is added and mixed evenly, the temperature is raised to 80-100° C. and stirred for reaction for 4-8 hours, filtered, washed, and dried to obtain the chlorinated paraffin-composite montmorillonite high-efficiency flame retardant.

10. The method for preparing the high-efficiency flame retardant of chlorinated paraffin composite montmorillonite according to claim 9, characterized in that: The dispersion medium is at least one of water, ethanol or methanol, and the content of the montmorillonite after being evenly dispersed in the dispersion medium is 1-5wt%.

11. Use of the high-efficiency flame retardant of the chlorinated paraffin composite montmorillonite according to any one of claims 1 to 8 in flame-retardant plastics.

12. The use of the high-efficiency flame retardant in flame-retardant plastics according to claim 11, characterized in that: The flame retardant plastic comprises a polymer matrix and the high-efficiency flame retardant.

13. The use of the high-efficiency flame retardant in flame-retardant plastics according to claim 12, characterized in that: The polymer matrix is ​​at least one of PE, PP, PA, PC, PBT or ABS.

14. The use of the high-efficiency flame retardant in flame-retardant plastics according to claim 12, characterized in that: The amount of the high-efficiency flame retardant is 1-20wt% of the polymer matrix.

Citation Information

Patent Citations

  • Physical bacteria resisting net liquid of human body and the producing technique

    CN101032498A

  • Preparation method for bifunctional-modified montmorillonite dispersion liquid

    CN102372274A

  • Method of positive ion currying work for leather

    CN1046561A

  • Dendritic modified montmorillonite flame retardant and preparation method thereof

    CN104710652A

  • Flame-retardant polycyclohexene carbonate nanometer composite material and preparation method thereof

    CN104987686A