Cross-linked mixed conductor film material and method for initiating polymerization and film formation on the surface of negative electrode particles

By designing a cross-linked mixed conductor film material on the surface of the alloy anode particles of the lithium ion battery, combined with the combined coating of the carbon intermediate layer and the mixed conductor outer layer, the problem of structural damage caused by the volume change of the alloy anode material during the charge and discharge process is solved, achieving It has high mechanical toughness and excellent electrical conductivity, significantly improving the cycle and rate performance of the battery.

CN117936745BActive Publication Date: 2024-10-22SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410118903.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-29
Publication Date
2024-10-22
Estimated Expiration
2044-01-29

AI Technical Summary

Technical Problem

The volume change of the lithium-ion battery alloy negative electrode material during the charge and discharge process causes the electrode structure to be damaged, the active material and the conductive agent lose electrical contact, and the common carbon coating layer is easy to crack and fall off during the cycle, affecting the battery performance.

Method used

By grafting polymer monomers on the surface of alloy negative electrode particles and initiating surface polymerization, the cross-linked structure and dual macromolecular chains are designed to form a cross-linked mixed conductor film material, which is combined with polybasic organic acids as cross-linking centers to achieve electronic and ion conduction. It has both performance and is coated with a combination of carbon intermediate layer and hybrid conductor outer layer to improve mechanical toughness and electrical conductivity.

Benefits of technology

The structural stability and electrochemical performance of the alloy anode material during the charge and discharge process are improved, the cycle performance and rate performance are significantly improved, the battery life is extended and the first Coulombic efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117936745B_ABST
    Figure CN117936745B_ABST
Patent Text Reader

Abstract

The present invention discloses a cross-linked mixed conductor film material and a method for initiating polymerization and film formation on the surface of alloy negative electrode particles. On the surface of alloy negative electrode material particles with large volume changes such as Si or Sn, Ge, Al, etc., an electronic conductive polymer monomer group is grafted to the surface of the particle material through surface modification, and a polybasic organic acid-terminated ion conductive polymer is synthesized and used as a doping acid for the electronic conductive polymer. The organic acid-terminated ion conductive polymer, the electronic conductive polymer monomer, and the surface-grafted particle material are polymerized in situ to obtain a mixed conductor-coated alloy negative electrode composite material. The film material of the present invention can achieve good lithium ion / electron conduction, adapt to volume changes during charging and discharging, and greatly improve the cycle performance and rate performance of the alloy negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lithium ion battery materials, and in particular relates to a cross-linked mixed conductor coating layer material suitable for lithium ion battery large expansion alloy negative electrode particles and a surface initiated polymerization film-forming method thereof. Background Art

[0002] Lithium-ion batteries have broad prospects in the fields of electric vehicles and energy storage technology due to their high energy density, high coulomb efficiency, and low self-discharge. In order to meet the requirements of high energy density, suitable electrode materials need to be designed. Alloy negative electrodes (silicon, tin, germanium, aluminum, etc.) can store lithium through alloying / de-alloying reactions with lithium ions and have extremely high theoretical capacity. Silicon has a wide range of sources and a moderate lithium insertion potential. The theoretical specific capacity at room temperature is as high as 3590 mAh / g (corresponding to Li 15 Si4) can significantly improve the battery energy density compared to commercial negative electrode material graphite (theoretical specific capacity 372 mAh / g).

[0003] However, during the charge and discharge process, the huge volume change of the alloy negative electrode will destroy the electrode structure, and the active material and the conductive agent will lose electrical contact, resulting in a decrease in capacity; the volume change during the cycle process destroys the solid electrolyte interface (SEI) on the surface of the active particles, and the SEI continuously destroys and reforms, rapidly consuming electrolyte and lithium ions. Some alloy particles have low intrinsic conductivity and their high current charge and discharge capabilities are limited. Carbon coating is a common method for improving alloy negative electrode materials, but carbon materials have poor flexibility, and the surface carbon coating is prone to cracking and falling off during pole piece rolling and battery cycling, affecting its performance.

[0004] Polymers have good flexibility and are easy to design their molecular structures to regulate their properties (electronic / ionic conductivity, mechanical properties, etc.). However, there is still the problem of how to design polymer electronic / ionic pathways and ensure the coating effect of the polymer. A single electronic conductive polymer or an uneven coating layer will affect the ion transport of the composite material. At the same time, common electronic conductive polymers are difficult to dissolve in water and conventional organic solvents, and it is not only difficult to form a uniform film on the surface of alloy negative electrode particles, but also difficult to ensure its adhesion stability on the surface. Therefore, the development of a mixed conductor coating material with excellent electronic / ionic mixed conductivity and a method to achieve uniform film formation and stable adhesion on the surface of alloy negative electrode materials is of great significance for the development of lithium-ion battery negative electrode materials with long life and high rate performance. Summary of the invention

[0005] The purpose of the present invention is to provide a cross-linked mixed conductor polymer film material and a method for uniformly coating the surface of alloy negative electrode particles. By grafting polymer monomers on the surface of alloy negative electrode particles and initiating surface polymerization, uniform conformal coating of the film material on the particle surface is achieved; by designing the cross-linked structure and the double macromolecular chain in the molecular structure, the mixed conductor film has high mechanical toughness and excellent electronic / lithium ion conductivity. This kind of film material tightly attached to the surface of the alloy particles can achieve good lithium ion / electron conduction, adapt to the volume change during the charge and discharge process, and greatly improve the cycle performance and rate performance of the alloy negative electrode material.

[0006] The main idea of ​​the present invention is to graft electronic conductive polymer monomers (aniline, pyrrole, thiophene molecules) onto the surface of silicon-based alloy negative electrode particles (nano silicon, micron silicon, porous silicon, silicon oxide, silicon-carbon composite materials, etc.) or Sn-based, Ge-based, Al-based alloy negative electrode material particles through surface modification, and after the end groups of ion conductive polymers are capped with polybasic organic acids, they are used as doping acids of electronic conductive polymers, and then the electronic conductive polymer monomers are polymerized by in-situ initiation to obtain a uniform mixed conductor coating film material (coating layer). The mixed conductor uses polybasic organic acids (phytic acid, camphorsulfonic acid, tannic acid, etc.) as the cross-linking center, and the ion conductive polymers (polyethylene oxide, polyethylene glycol, polyethylene glycol diglycidyl ether, polyacrylonitrile, lithiated polyacrylic acid, etc.) and organic acids are bonded through chemical reactions, and the surplus protons of the organic acids serve as acid dopants for electronic conductive polymers (polyaniline, polypyrrole, polydioxyethylthiophene, etc.); thus, the macromolecular network of the coating layer has mixed conductor properties. On the one hand, the polymer coating layer has good mechanical strength and interface viscosity, and is always wrapped around the alloy-based negative electrode material particles during the charge and discharge process to maintain its particle structure; on the other hand, the coating layer itself has good electronic and ion conductivity, which can achieve reversible lithium insertion and extraction cycles even under high current conditions. The composite material coated with the improved mixed conductor with the above advantages will have the characteristics of low specific surface area, high tap density, high conductivity, and stable cycle.

[0007] The cross-linked mixed conductor film material provided by the present invention is suitable for Si, Sn, Ge, and Al-based alloy negative electrode particles. For example, with silicon-based negative electrode particles as the matrix, for particles with a larger specific surface area (such as porous silicon and nano silicon), carbon coating is first performed or micron particles with a lower specific surface area are formed by granulation, and then a uniformly coated and firmly adhered mixed conductor coating layer is formed by in-situ polymerization; for particles with a lower specific surface area (such as micron silicon and silicon oxide), the surface of the mixed conductor film is directly polymerized and coated. The mass ratio of silicon, carbon intermediate layer, and mixed conductor outer layer is (5%~95%) (0~50%) (5~50%).

[0008] The cross-linked mixed conductor film material provided by the present invention is coated on the surface of the alloy negative electrode particles of the lithium ion battery, and is composed of a carbon middle layer and a mixed conductor outer layer, and the mass ratios of the alloy negative electrode particles, the carbon middle layer and the mixed conductor outer layer are (55%~95%): (0%~30%): (5%~15%) respectively; the alloy negative electrode particles are one of the lithium ion battery large expansion alloy negative electrode particles such as Si, Sn, Ge, Al, etc.; the mixed conductor outer layer is formed by in-situ polymerization and cross-linking of ion conductive polymers and electronic conductive polymer monomers on the surface of the alloy negative electrode particles.

[0009] Furthermore, the ion conductive polymer is selected from one of polyethylene oxide, polyethylene glycol, polyethylene glycol diglycidyl ether, polyacrylonitrile, and lithiated polyacrylic acid; the electronic conductive polymer is selected from one of polyaniline, polypyrrole, poly(ethylenedioxythiophene), and poly(3,4-diethylenedioxythiophene).

[0010] The method for initiating polymerization of the cross-linked mixed conductor film material on the surface of alloy negative electrode particles provided by the present invention comprises the following steps:

[0011] (1) For alloy negative electrode particles with a large specific surface area, carbon coating or granulation is used to form micron particles with a low specific surface area; for alloy negative electrode particles with a low specific surface area, this step is not required;

[0012] The alloy negative electrode material particles are mixed with a carbon source, and the carbon source is coated by a chemical method, wherein the mass ratio of the carbon source to the alloy negative electrode material particles is 1:(1-9); and then carbonized in an inert atmosphere to obtain a composite material S1;

[0013] (2) The composite material S1 is surface modified with a surface modifier, so that the comonomer compound of the electronic conductive polymer is grafted onto the surface of the material to obtain the composite material S2, so that the subsequent polymerization reaction occurs on the surface of the particles, and the adhesion of the coating layer on the surface of the particles is increased through chemical bridging, thereby achieving uniform and conformal coating;

[0014] (3) An organic acid with multiple functional groups is used as a cross-linking center to induce the terminal functional groups of the ion-conductive polymer to react and bond with the organic acid to obtain an organic acid grafted onto the ion-conductive polymer; wherein the molar ratio of the organic acid to the ion-conductive polymer is 1:(0.5~2).

[0015] (4) The composite material S2 is polymerized with the electronic conductive polymer monomer and the ion conductive polymer grafted organic acid under appropriate conditions, wherein the mass ratio of the composite material S2 to the electronic conductive polymer monomer is 1:(0.05-0.2), and the molar ratio of the electronic conductive polymer monomer, the ion conductive polymer grafted organic acid, and the oxidant is 1:(0.5-2):1. After filtering and drying, a composite material coated with a mixed conductor membrane is obtained, wherein the cross-linked mixed conductor membrane material is uniformly coated on the surface of the composite material particles.

[0016] In the above method, the silicon-based negative electrode particles can also be replaced by Sn-based, Ge-based, Al-based and other lithium-ion battery large expansion alloy negative electrode particles.

[0017] In the above method, further, the alloy negative electrode material particles used in step (1) are selected from at least one of nano silicon, porous silicon, micro silicon and silicon dioxide.

[0018] In the above method, further, the carbon source in step (1) is an organic material with a high carbon content or a mixture thereof, preferably at least one selected from asphalt, phenolic resin, polyvinyl chloride, glucose, and citric acid.

[0019] In the above method, further, the chemical method in step (1) can be selected from spray drying or rotary evaporation; the carbonization temperature is 600-900 °C, and the carbonization heating rate is 5-10 °C / min; the inert atmosphere is argon, or a mixture of argon and hydrogen, or a mixture of nitrogen and hydrogen.

[0020] In the above method, further, the surface modification method in step (2) is: mixing a silane coupling agent, a composite material S1 and a solvent, reacting at 80°C for 2 hours, and grafting the active group (of the silane coupling agent) onto the silicon surface, wherein the mass ratio of the composite material S1 to the silane coupling agent is 1:(0.01-0.02), and the solvent is a mixed solvent of water and ethanol; then mixing the reaction product with a comonomer compound of an electronic conductive polymer (the compound can be connected with the silane coupling agent and can be involved in the subsequent copolymerization with the electronic conductive polymer monomer) and a solvent for reaction, wherein the solvent is a mixed solvent of water and ethanol, wherein the molar ratio of the silane coupling agent to the comonomer compound of the electronic conductive polymer is (0.8-1.2):1, the reaction temperature is 80°C-120°C, and the reaction time is 3-8 hours.

[0021] Preferably, the silane coupling agent is selected from at least one of vinyl triethoxysilane, vinyl trimethoxysilane, and vinyl tri(β-methoxyethoxy)silane; and the comonomer compound of the electronic conductive polymer is selected from at least one of m-phenylenediamine, p-phenylenediamine, triphenylamine, 2-pyrrolcarboxylic acid, and 3-pyrrolcarboxaldehyde.

[0022] In the above method, further, in step (3), the ion conductive polymer is selected from one of polyethylene oxide, polyethylene glycol, polyethylene glycol diglycidyl ether, polyacrylonitrile, and lithiated polyacrylic acid; and the organic acid is selected from at least one of phytic acid, camphorsulfonic acid, and tannic acid.

[0023] In the above method, further, in step (3), the ion conductive polymer and the organic acid are stirred and reacted at a temperature of 120 to 150° C. for 2 to 4 hours to obtain the ion conductive polymer grafted with the organic acid.

[0024] In the above method, further, the particle size of the obtained silicon-mixed conductor composite material is about 1-5 μm, the thickness of the carbon coating layer is 10-20 nm, and the thickness of the polymer coating layer is about 10-20 nm.

[0025] In the above method, further, the electronic conductive polymer monomer in step (4) is selected from one of aniline, pyrrole, 3,4-diethylenedioxythiophene, etc., and is the same type of organic matter as the comonomer compound of the electronic conductive polymer selected in step (2). For example, if an aniline comonomer is selected in step (2), aniline is selected in step (4); if a pyrrole comonomer is selected in step (2), pyrrole is selected in step (4); if a thiophene comonomer is selected in step (2), thiophene is selected in step (4); the selected oxidant is preferably ammonium persulfate.

[0026] In the above method, further, in step (4), the oxidant solution is slowly added to the mixed solution of S2 powder, electronic conductive polymer monomer, and ion conductive polymer grafted organic acid.

[0027] The present invention also provides the use of the cross-linked mixed conductor film material in lithium-ion batteries. Preferably, the application is as a negative electrode material with excellent cycle and rate performance of lithium-ion batteries.

[0028] The principle of the present invention is as follows: first, a silane coupling agent is used to react on the surface of the alloy negative electrode to introduce active groups (such as epoxy groups, etc.) on its surface; then, the comonomer compound of the electronic conductive polymer is induced to react with the active groups in the silane coupling agent (such as an amino group in m-phenylenediamine reacts with the epoxy group), thereby realizing the grafting of electronic conductive polymer monomers on the surface of silicon particles, and initiating polymerization on the surface of active particles in the subsequent polymerization process. At the same time, the terminal functional groups of the ion conductive polymer react with the polybasic organic acid (such as the esterification reaction between the terminal hydroxyl group of polyethylene oxide and part of the phosphate group in phytic acid), so that the ion conductive polymer forms a polybasic organic acid terminal group, and the remaining acid groups in the polybasic organic acid can be in-situ doped into the electronic conductive polymer molecular chain. In this way, in-situ surface polymerization realizes the formation of an electronic / ion dual-conducting polymer cross-linking network while realizing the uniform and conformal growth of the polymer coating layer on the surface of the alloy negative electrode particles.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The method of the present invention realizes conformal and uniform coating of the electron-ion dual-conducting polymer layer on the surface of the particle material by surface-initiated polymerization; before coating, the polymer monomer group is grafted on the surface of the particle material to initiate the subsequent in-situ surface polymerization process and establish a strong chemical bond connection between the coating layer and the particle, thereby avoiding self-agglomeration of the polymer during the polymerization process and ensuring the stability of the material structure during the cycle. In the mixed conductor membrane material, with polybasic organic acid as the cross-linking center, the electronic conductive polymer and the ion conductive polymer form a three-dimensional penetrating, chemically cross-linked macromolecular network, thereby forming a conformal and uniform polymer modification layer with good mechanical and electrochemical properties on the surface of the alloy negative electrode particle.

[0031] 2. Compared with polymers or carbon materials with single properties, the cross-linked film layer of the electronic and ion dual-conducting polymer in the present invention takes into account both mechanical toughness and electronic ion conductivity. The cross-linked structure combines the ion conductive polymer and the electronic conductive polymer into a three-dimensional molecular network connected by chemical bonds (rather than a simple physical mixture), giving the polymer good toughness and strength, better adapting to particle expansion and inhibiting the cracking and pulverization of negative electrode particles while maintaining the stability of the electron / ion path, thereby improving the cycle performance and rate performance of the silicon-based negative electrode.

[0032] 3. The surface coating film technology described in the present invention can also significantly reduce the specific surface area of ​​alloy negative electrode materials, avoid direct contact between the alloy negative electrode and the electrolyte, and improve the first coulombic efficiency of large-capacity negative electrode materials. The prepared mixed conductor-coated silicon-based composite material has improved first efficiency, gram capacity, cycle life, rate performance, etc. compared with the current conventional graphite or silicon-carbon composite negative electrode materials.

[0033] 4. The raw material cost required for the present invention is low; the preparation equipment and process are simple, the reaction temperature is low and easy to control, and it is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is the cycle curve of the mixed conductor-coated silicon-based composite material prepared in Example 1 at a current density of 500 mA / g;

[0035] Figure 2 The scanning electron microscope (SEM) morphology (a) and energy dispersive spectrometer (EDS) element distribution diagram (b) of the mixed conductor-coated silicon-based composite material prepared in Example 1

[0036] Figure 3 The transmission electron microscope (TEM) morphology image (a) and EDS element distribution images (b, c) of the mixed conductor-coated silicon-based composite material prepared in Example 1;

[0037] Figure 4 The SEM morphology of the mixed conductor-coated silicon-based composite material electrode prepared in Example 1 after cycling (a is a 2k-fold SEM photo, and b is a 10k-fold SEM local magnified photo);

[0038] Figure 5 1 is the cycle curve of the silicon-based composite material with different silicon and mixed conductor ratios prepared in Example 4 at a current density of 500 mA / g;

[0039] Figure 6 The rate performance comparison of micron silicon, polyaniline coated micron silicon, and mixed conductor coated micron prepared in Example 5;

[0040] Figure 7 The cycle curve of the carbon-coated silicon-based negative electrode material prepared in Comparative Example 1 at a current density of 500 mA / g;

[0041] Figure 8 The SEM morphology of the electrode of the carbon-coated silicon-based negative electrode material prepared in Comparative Example 1 after cycling (a is a 2k-fold SEM photo and b is a 10k-fold SEM local magnified photo);

[0042] Fig. 9 Comparison of the cycle performance of the mixed conductor silicon-based material coated with the surface modified and the mixed conductor silicon-based material coated directly without surface modification prepared in Comparative Example 2;

[0043] Fig.10 This is a SEM photograph of the mixed conductor silicon-based material directly coated without surface modification prepared in Comparative Example 2. DETAILED DESCRIPTION

[0044] The present invention is further explained below in conjunction with specific examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above invention content.

[0045] Example 1

[0046] (1) Add 250 mg of asphalt into a mixed solvent of 5 ml of quinoline and 20 ml of n-decane and stir to dissolve, then add 500 mg of porous silicon and stir to mix to obtain dispersion A, and perform rotary evaporation at 130 °C for 2 hours with a vacuum degree of -0.09; collect powder B after the solvent evaporation is completed; place powder B in a tubular furnace and perform carbonization treatment in a high-purity argon atmosphere at a heating rate of 5 °C / min, keep the temperature at 300 °C for 1 hour, then heat to 900 °C and keep the temperature constant for 3 hours, and naturally cool to room temperature to obtain silicon-carbon composite particles S1;

[0047] (2) Mix 9 ml of ethanol and 1 ml of deionized water in a reagent bottle, add 200 μl of silane coupling agent, and add 100 μl of glacial acetic acid to adjust the solution to pH = 5.5, let it stand for 15 min, and obtain a mixed solution C; take 20 mg of m-phenylenediamine and dissolve it in 2 ml of water to obtain a solution D; take 200 μl of solution C and mix it with 200 mg of composite material S1 in a beaker, add 5 ml of water to disperse the particles, and react at 80 ° C in a vacuum for 2 hours to obtain dry powder E, then add 200 μl of solution D, add 5 ml of water to disperse the particles, and react at 120 ° C in a vacuum for 8 hours to obtain a surface-modified silicon-carbon composite material S2;

[0048] (3) 5 g of polyethylene oxide and 4.71 g of phytic acid aqueous solution (70% mass concentration) were stirred in an oil bath at 130 °C for 4 hours to obtain polyethylene oxide-phytate;

[0049] (4) Add 20 ml of water to the polyethylene oxide-phytate obtained in step (3), stir for 2 hours to dissolve, and obtain a polyethylene oxide-phytate solution; mix 100 mg of the composite material S2 with 20 μl of aniline and 500 μl of the polyethylene oxide-phytate solution in a beaker, and add 5 ml of deionized water to dissolve, to obtain a dispersion F; take 49 mg of ammonium persulfate in a sample bottle, add 3 ml of water to dissolve, and obtain a solution G; under the condition of a 4°C ice water bath, add solution G dropwise to the dispersion F, wait for the reaction to occur for 6 hours, filter the solution after the reaction is complete, wash with deionized water and ethanol to remove the monomers and oligomers that have not reacted completely, and dry it in a vacuum drying oven at 80°C for 12 hours to obtain a mixed conductor-coated silicon-based composite material.

[0050] The composite material of Example 1 was mixed with carbon black as a conductive agent and sodium carboxymethyl cellulose as an adhesive in a ratio of 8:1:1 to form electrodes, and a button cell was assembled with a lithium sheet as a counter electrode, and a cycle performance test was performed. Figure 1 As shown, the battery was first activated for three cycles at a current density of 50 mA / g, with the first discharge specific capacity of 1652.5 mA h / g, the first charge specific capacity of 1366.3 mAh / g, and the first coulombic efficiency of 82.7%; the charge and discharge cycle was carried out at a current density of 500 mA / g, with a capacity of 1060.2 mAh / g. After 200 cycles at this current density, the reversible specific capacity of the material was 868.8 mA h / g, and its capacity retention rate was 82.0%.

[0051] Attached Figure 2 The SEM (a) and EDS (b) characterization analysis of the mixed conductor-coated silicon-carbon material prepared in this embodiment are shown, showing that the particles are dense, the surface is smooth, and the silicon and carbon elements are evenly distributed. Figure 3 TEM and EDS characterization analysis of the material show that the mixed conductor coating layer is about 20-40 nm thick and is evenly coated on the surface of the particles. Its existence plays a significant role in improving the cycling performance of silicon. Figure 4 This is a SEM photo of the electrode sheet after charge and discharge cycles. The spherical morphology of the particles in the electrode is complete, indicating that the mixed conductor coating plays a key role in suppressing the breakage and pulverization of silicon particles and stabilizing the electrode structure during the cycle.

[0052] Example 2

[0053] (1) 500 mg of porous silicon and 250 mg of glucose were mixed in 100 ml of deionized water, placed in a 60 °C water bath environment for mixing and stirring, to obtain dispersion A and spray dried; the inlet temperature of the spray dryer was set to 200 °C, the outlet temperature was set to 80 °C, and the peristaltic pump was set to 10 ml / min. After the spray drying was completed, powder B was collected; B was placed in a tubular furnace and carbonized in a high-purity argon atmosphere at a heating rate of 5 °C / min, kept at 300 °C for 1 hour, then heated to 800 °C and kept constant for 3 hours, and naturally cooled to room temperature to obtain silicon-carbon composite particles S1;

[0054] (2) Mix 9 ml of ethanol and 1 ml of deionized water in a reagent bottle, add 200 μl of coupling agent, and add 100 μl of glacial acetic acid to adjust the solution to pH = 5.5, let it stand for 15 min, and obtain a mixed solution C; take 20 mg of m-phenylenediamine and dissolve it in 2 ml of water to obtain a solution D; take 200 μl of solution C and mix it with 200 mg of composite material S1 in a beaker, add 5 ml of water to disperse the particles, and react at 80 ° C in a vacuum for 2 hours to obtain dry powder E, then add 200 μl of solution D, add 5 ml of water to disperse the particles, and react at 120 ° C in a vacuum for 8 hours to obtain a surface-modified silicon-carbon composite material S2;

[0055] (3) 5 g of polyethylene oxide and 4.71 g of phytic acid aqueous solution (70% concentration) were stirred in an oil bath at 130 °C for 4 hours to obtain polyethylene oxide-phytate;

[0056] (4) Add 20 ml of water to the polyethylene oxide-phytate obtained in step (3) and stir for 2 hours to dissolve to obtain a polyethylene oxide-phytate solution. Mix 100 mg of composite material S2 with 20 μl of aniline and 500 μl of polyethylene oxide-phytate solution in a beaker, add 5 ml of deionized water to dissolve, and obtain dispersion F; take 49 mg of ammonium persulfate in a sample bottle and add 3 ml of water to dissolve to obtain solution G; under the condition of a 4°C ice water bath, add solution G dropwise to dispersion F, wait for 6 hours to react, filter the solution after the reaction is complete, wash the unreacted monomers and oligomers with deionized water and ethanol, and dry it in a vacuum drying oven at 80°C for 12 hours to obtain a mixed conductor-coated silicon-based conductor composite material.

[0057] The composite material of Example 2 was prepared into electrodes with the conductive agent carbon black and the adhesive sodium carboxymethyl cellulose in a ratio of 8:1:1, and a button cell was assembled with a lithium sheet as the counter electrode, and the cycle performance test was performed. The battery was first activated for three cycles at a current density of 50 mA / g, with the first discharge specific capacity of 1477.6 mA h / g, the first charge specific capacity of 1230.3 mA h / g, and the first coulomb efficiency of 83.26%; the charge and discharge cycle was performed at a current density of 500 mA / g, and the capacity was 1069.0 mA h / g. After 200 cycles at this current density, the reversible specific capacity of the material was 814.8 mA h / g, and its capacity retention rate was 76.2%.

[0058] Example 3

[0059] (1) 4 g of nano-silicon and 2 g of phenolic resin were mixed in 200 ml of deionized water, stirred at room temperature, and then oxalic acid precipitant was added. The mixture was centrifuged, dried, and ball-milled to obtain powder A. 4 g of powder A, 1 g of citric acid, and 1 g of polyvinyl pyrrolidone were dissolved in 20 ml of deionized water, stirred to obtain a uniform dispersion, and spray-dried. The inlet temperature of the spray dryer was set to 200 °C, the outlet temperature was set to 80 °C, and the peristaltic pump was set to 32 mI / min. After the spray drying was completed, powder B was collected. B was placed in a tubular furnace and subjected to a recovery treatment in a high-purity argon atmosphere. The temperature was kept at 300 °C for 1 hour at a heating rate of 5 °C / min, then the temperature was raised to 800 °C and kept constant for 3 hours. After naturally cooling to room temperature, silicon-carbon composite particles S1 were obtained.

[0060] (2) Mix 9 ml of ethanol and 1 ml of deionized water in a reagent bottle, add 200 μl of coupling agent, and add 100 μl of glacial acetic acid to adjust the solution to pH = 5.5, let it stand for 15 min, and obtain a mixed solution C; take 20 mg of m-phenylenediamine and dissolve it in 2 ml of water to obtain a solution D; take 200 μl of solution C and mix it with 200 mg of composite material S1 in a beaker, add 5 ml of water to disperse the particles, and react at 80 ° C in a vacuum for 2 hours to obtain dry powder E, then add 200 μl of solution D, add 5 ml of water to disperse the particles, and react at 120 ° C in a vacuum for 8 hours to obtain a surface-modified silicon-carbon composite material S2;

[0061] (3) 5 g of polyethylene oxide and 4.71 g of phytic acid aqueous solution (70% concentration) were stirred in an oil bath at 130 °C for 4 hours to obtain polyethylene oxide-phytate;

[0062] (4) Add 20 ml of water to the polyethylene oxide-phytate obtained in step (3) and stir for 2 hours to dissolve to obtain a polyethylene oxide-phytate solution. Mix 100 mg of composite material S2 with 20 μl of aniline and 500 μl of polyethylene oxide-phytate solution in a beaker, add 5 ml of deionized water to dissolve, and obtain dispersion F; take 49 mg of ammonium persulfate in a sample bottle and add 3 ml of water to dissolve to obtain solution G; add solution G dropwise to dispersion F under the condition of a 4°C ice water bath, wait for the reaction for 6 hours, filter the solution after the reaction is complete, wash the unreacted monomers and oligomers with deionized water and ethanol, and dry it in a vacuum drying oven at 80°C for 12 hours to obtain a mixed conductor-coated silicon-based composite material.

[0063] The composite material of Example 3 was prepared into electrodes with the conductive agent carbon black and the adhesive sodium carboxymethyl cellulose in a ratio of 8:1:1, and a button cell was assembled with a lithium sheet as the counter electrode, and the cycle performance test was performed. The battery was first activated for three cycles at a current density of 50 mA / g, and the first discharge specific capacity was 2011.1 mA h / g, the first charge specific capacity was 1674.2 mA h / g, and the first coulomb efficiency was 83.25%; the charge and discharge cycle was performed at a current density of 500 mA / g, and the capacity was 1416.4 mA h / g. After 80 cycles at this current density, the reversible specific capacity of the material was 1197.2 mAh / g, and its capacity retention rate was 84.5%.

[0064] Example 4

[0065] (1) Mix 9 ml of ethanol and 1 ml of deionized water in a reagent bottle, then add 200 μl of coupling agent and 100 μl of glacial acetic acid, and let stand for 15 min to obtain a mixed solution A; dissolve 20 mg of m-phenylenediamine in 2 ml of water to obtain a solution B; mix 600 μl of solution A with 600 mg of porous silicon in a beaker, add 5 ml of water to disperse the particles, and react at 80 °C in a vacuum environment for 2 hours to obtain a dry powder C, then add 600 μl of solution B, add 5 ml of water to disperse the particles, and react at 120 °C in a vacuum environment for 8 hours to obtain surface-modified porous silicon S1;

[0066] (2) 5 g of polyethylene oxide and 4.71 g of phytic acid aqueous solution (70% concentration) were stirred in an oil bath at 130 °C for 4 hours to obtain polyethylene oxide-phytate;

[0067] (3) Add 20 ml of water to the obtained polyethylene oxide-phytate and stir for 2 hours to dissolve to obtain a polyethylene oxide-phytate solution. Silicon composite materials S2 with different silicon and cross-linked mixed conductor ratios (different cross-linked mixed conductor coating material content) were prepared on the basis of the surface-modified porous silicon S1. The proportion of the mixed conductor coating layer in the composite material was adjusted by controlling the ratio of silicon:aniline. The preparation conditions for the silicon:aniline mass ratio of 10:1 were as follows:

[0068] 10 μl of aniline, 250 μl of polyethylene oxide phytate solution and 5 ml of deionized water were mixed, and 100 mg of composite material S2 was added and stirred to form dispersion D; 24.5 mg of ammonium persulfate was dissolved in 5 ml of deionized water to obtain solution E; solution E was added dropwise to dispersion D in an ice water bath at 4°C, and the reaction was allowed to proceed for 6 hours. After the reaction was completed, the solution was filtered, and the unreacted monomers and oligomers were washed with deionized water and ethanol, and dried in a vacuum drying oven at 80°C for 12 hours to obtain a mixed conductor-coated porous silicon composite material, which was recorded as P1.

[0069] The proportion of mixed conductors in the composite material was changed by controlling the ratio of silicon to polymer monomers. According to the same method, the mass ratio of porous silicon to aniline was changed, and the mass ratio of polyethylene oxide-phytate, ammonium persulfate and aniline was kept unchanged to prepare composite materials with a mass ratio of porous silicon to aniline of 2.5:1, 10:3, and 5:1, which were recorded as P2, P3, and P4 respectively.

[0070] The composite materials with four different mixed conductor contents obtained in Example 4 were mixed with conductive agent carbon black and adhesive sodium carboxymethyl cellulose in a ratio of 8:1:1 to form electrodes, and lithium sheets were used as counter electrodes to assemble button-type batteries, and the cycle performance test was carried out. Figure 5 This is the battery cycle test curve in this embodiment. The battery was first activated for three cycles at a current density of 50 mA / g, and then cycled for 200 cycles at a current density of 500 mA / g. It was found through testing that after 100 cycles, the capacity retention rates of P1, P2, P3, and P4 were 17.9%, 70.13%, 47.5%, and 21.64%, respectively. After 200 cycles, the capacity retention rates of P1, P2, P3, and P4 were 5.18%, 55.79%, 13.15%, and 8.51%, respectively.

[0071] Comparing the four groups of batteries, the experimental group with a moderate content of mixed conductor in the composite material has the best cycling performance, indicating that the content of the mixed conductor should be controlled within a certain range. A too thick mixed conductor layer will inhibit the transmission of electrons / ions, while a too thin coating layer is not enough to solve the cracking and powdering problem of silicon during the cycling process.

[0072] Example 5

[0073] (1) Mix 9 ml of ethanol and 1 ml of deionized water in a reagent bottle, then add 200 μl of coupling agent and 100 μl of glacial acetic acid, and let stand for 15 min to obtain a mixed solution A; dissolve 20 mg of m-phenylenediamine in 2 ml of water to obtain a solution B; mix 600 μl of solution A with 600 mg of microsilicon in a beaker, add 5 ml of water to disperse the particles, and react at 80°C in a vacuum environment for 2 hours to obtain a dry powder C, then add 600 μl of solution B, add 5 ml of water to disperse the particles, and react at 120°C in a vacuum environment for 8 hours to obtain surface-modified microsilicon S1;

[0074] (2) 5 g of polyethylene oxide and 4.71 g of phytic acid aqueous solution (70% concentration) were stirred in an oil bath at 130 °C for 4 hours to obtain polyethylene oxide-phytate;

[0075] (3) Add 23.3 mg of aniline and 50 mg of polyethylene oxide phytate to 5 ml of deionized water and stir to form a clear solution D. Then add 400 mg of micron silicon S1 and disperse it ultrasonically for 20 minutes. Dissolve 57 mg of ammonium persulfate in 5 ml of deionized water to form solution E. Add solution E dropwise into dispersion D in an ice-water bath at 4°C and wait for the reaction to occur for 6 hours. After the reaction is complete, filter the solution and wash away the unreacted monomers and oligomers with deionized water and ethanol. Dry the solution in a vacuum drying oven at 80°C for 12 hours to obtain a mixed conductor-coated micron silicon composite material.

[0076] As a control group, no polyethylene oxide phytate was added during the preparation process, and other conditions were the same to obtain a polyaniline-coated micro-silicon composite material.

[0077] The micron silicon, polyaniline (single electron conductive polymer) coated micron silicon composite materials, and mixed conductor coated micron silicon composite materials of this embodiment were respectively mixed with conductive agent carbon black and adhesive sodium carboxymethyl cellulose in a ratio of 8:1:1 to make electrodes, and button cells were assembled with lithium sheets as counter electrodes, and cycle performance tests were carried out, marked as B1, B2, and B3 respectively, and rate performance tests were carried out.

[0078] Attached Figure 6The figure is the battery rate test curve. The capacity of micro-silicon (battery B1) has rapidly decayed in the first 10 cycles of small current (0.1, 0.2 A / g) tests. When the current increases to 0.5 A / g, the capacity is less than 100 mA h / g, indicating that most of the micro-silicon has lost electronic contact. The polyaniline-coated micro-silicon composite material (battery B2) exerts reversible capacities of 2603.7, 2301.4, 2083.3, 1758.2, 1370.1, and 997.8 at 0.1, 0.2, 0.5, 1, 2, and 4 A / g, respectively. When the current is adjusted back from 4 A / g to 0.5 A / g, the capacity recovers to 1812.4 mA h / g. The mixed conductor coated micron silicon composite material (battery B3) exhibited reversible capacities of 2794.8, 2771.3, 2619.5, 2356.8, 2016.6 and 1632.7 mA h / g at 0.1, 0.2, 0.5, 1, 2 and 4 A / g, respectively. When the current was adjusted back from 4 A / g to 0.5 A / g, the capacity recovered to 2384.6 mAh / g, which was 234.9 mA h / g lower than the capacity at 0.5 A / g in the 20-cycle rate test. This shows that the mixed conductor coated micron silicon has better rate performance, and the capacity attenuation is small under the conditions of large current rapid charge and discharge. This shows that the mixed conductor coating layer composed of polyaniline and polyethylene glycol has a significant effect on improving the high-rate performance of the battery compared with a single electronic conductive polymer due to the introduction of ion conductive groups.

[0079] Comparative Example 1

[0080] (1) Add 250 mg of asphalt into a mixed solvent of 5 ml of quinoline and 20 ml of n-decane and stir to dissolve, then add 500 mg of porous silicon and stir to mix, obtain dispersion A and perform rotary evaporation at 130 °C for 2 hours with a vacuum degree of -0.09; collect powder B after the solvent evaporation; place B in a tubular furnace and perform carbonization treatment in a high-purity argon atmosphere at a heating rate of 5 °C / min, keep the temperature at 300 °C for 1 hour, then heat to 900 °C and keep the temperature constant for 3 hours, and naturally cool to room temperature to obtain silicon-carbon composite particles S1;

[0081] (2) The composite material S1 of this comparative example 1 was mixed with carbon black as a conductive agent and sodium carboxymethyl cellulose as an adhesive in a ratio of 8:1:1 to form electrodes, and a button cell was assembled with a lithium sheet as a counter electrode, and a cycle performance test was performed. Figure 7The battery cycle performance curve of this comparative example is as follows: after three activation cycles at a current density of 50 mA / g, the first discharge capacity is 1722.6 mA h / g, the first charge capacity is 1245.9 mA h / g, and the first coulombic efficiency is 72.3%; after 100 cycles of charge and discharge at a current density of 500 mA / g, the reversible capacity of the material is 651.2 mA h / g, and the capacity retention rate is 43.0%. Figure 8 The SEM characterization analysis of the electrode after 100 cycles shows that there are obvious cracks on the electrode surface and the spherical particles are completely broken, indicating that a single carbon layer is not enough to suppress the volume change of the silicon negative electrode during the cycle. Figure 4 The silicon particles coated with the mixed conductor in Example 1 shown in the figure have a complete structure after cycling, which illustrates the key role of the mixed conductor in suppressing the breakage and pulverization of silicon particles and stabilizing the electrode structure.

[0082] Comparative Example 2

[0083] (1) 800 mg of porous silicon and 250 mg of glucose were mixed in 150 ml of deionized water, and the mixture was placed in a 60 °C water bath for mixing and stirring to obtain a dispersion A, which was then spray dried. The inlet temperature of the spray dryer was set to 200 °C, the outlet temperature was set to 80 °C, and the peristaltic pump was set to 10 ml / min. After the spray drying was completed, powder B was collected. B was placed in a tubular furnace and carbonized in a high-purity argon atmosphere. The temperature was kept at 300 °C for 1 hour at a heating rate of 5 °C / min, and then the temperature was raised to 800 °C and kept constant for 3 hours. After naturally cooling to room temperature, silicon-carbon composite particles S1 were obtained.

[0084] (2) 5 g of polyethylene oxide and 4.71 g of phytic acid aqueous solution (70% concentration) were stirred in an oil bath at 130 °C for 4 hours to obtain polyethylene oxide-phytate;

[0085] (3) Take 40 μl of aniline and 1000 μl of polyethylene oxide-phytate and place them in a beaker, add 100 mg of composite material S1 to one of them, and add 5 ml of deionized water to dissolve it to obtain dispersion C; take 98 mg of ammonium persulfate in a sample bottle and add it to 3 ml of water to dissolve it to obtain solution D; under the condition of a 4°C ice water bath, add solution D dropwise into dispersion C, wait for the reaction for 6 hours, filter the two solutions after the reaction is complete, wash away the unreacted monomers and oligomers with deionized water and ethanol, and dry them in a vacuum drying oven at 80°C for 12 hours to obtain the unsurface-modified mixed conductor-coated silicon-based negative electrode material S2.

[0086] As a comparison, the surface of silicon-carbon composite particles was modified:

[0087] Mix 9 ml of ethanol and 1 ml of deionized water in a reagent bottle, then add 200 μl of coupling agent and 100 μl of glacial acetic acid, and let stand for 15 min to obtain a mixed solution E; dissolve 20 mg of m-phenylenediamine in 2 ml of water to obtain a solution F; mix 600 μl of solution E with 600 mg of composite material S1 in a beaker, add 5 ml of water to disperse the particles, react at 80°C in a vacuum for 2 hours to obtain dry powder G, then add 600 μl of solution F, add 5 ml of water to disperse the particles, and react at 120°C in a vacuum environment for 8 hours to obtain surface-modified silicon-carbon composite particles S3;

[0088] The subsequent preparation steps are consistent with those in Comparative Examples (2)-(3), and a surface-modified mixed conductor-coated silicon-based negative electrode material S4 is obtained.

[0089] The composite material of comparative example 2 was mixed with carbon black as a conductive agent and sodium carboxymethyl cellulose as an adhesive in a ratio of 8:1:1 to form electrodes, and a button cell was assembled with a lithium sheet as a counter electrode, and a cycle performance test was performed. Fig. 9 The battery cycle performance curve in this comparative example. After 50 cycles, the capacity retention rate of the unmodified mixed conductor coated silicon-based negative electrode material is 60.3%, and the cycle retention rate of the surface modified mixed conductor composite material is 91.37%. It can be seen that after surface modification, the cycle performance of the obtained mixed conductor coated silicon material is significantly improved. Fig.10 The SEM characterization analysis of the unsurface-modified mixed conductor-coated silicon-based negative electrode material prepared in this comparative example shows that the polymer agglomeration phenomenon is serious and the surface of the silicon particles is not effectively coated, which indicates that surface modification has a significant improvement in improving the polymer coating effect, thereby improving the cycle performance of the silicon negative electrode.

Claims

1. A negative electrode material for a lithium-ion battery, It is characterized in that The negative electrode material of the lithium-ion battery comprises negative electrode particles, and a cross-linked mixed conductor film material coated on the surface of the negative electrode particles, wherein the cross-linked mixed conductor film material is composed of a carbon middle layer and a mixed conductor outer layer, and the mass percentages of the negative electrode particles, the carbon middle layer, and the mixed conductor outer layer are (55% to 95%): (0% to 30%): (5% to 15%), respectively; the mixed conductor outer layer is formed by in-situ polymerization and cross-linking of ion conductive polymers and electronic conductive polymer monomers on the surface of the negative electrode particles; The lithium ion battery negative electrode material is prepared by the following method: (1) If the negative electrode particles are porous silicon or nano silicon, they are first carbon coated to form micron particles, wherein the carbon coating method is to mix the negative electrode particles with a carbon source, and to coat the carbon source by a chemical method, wherein the mass ratio of the carbon source to the negative electrode particles is 1:(1-9); and then carbonized in an inert atmosphere; if the negative electrode particles are micron silicon or silicon oxide, this step is not required; Material S1 is obtained through the above steps; (2) The material S1 is surface modified by using a surface modifier, so that the comonomer compound of the electronic conductive polymer is grafted onto the surface of the material to obtain the composite material S2; the surface modification method is: a silane coupling agent, material S1 and a solvent are mixed, and the reaction is carried out at 80°C for 2 hours to graft the active group onto the silicon surface, wherein the mass ratio of the material S1 to the silane coupling agent is 1:(0.01-0.02), and the solvent is a mixed solvent of water and ethanol; then the reaction product is mixed with the comonomer compound of the electronic conductive polymer and a solvent for reaction, wherein the solvent is a mixed solvent of water and ethanol, wherein the molar ratio of the silane coupling agent to the comonomer compound of the electronic conductive polymer is (0.8-1.2):1, the reaction temperature is 80°C-120°C, and the reaction time is 3-8 hours; (3) Using an organic acid with multiple functional groups as a crosslinking center to induce the terminal functional groups of the ion-conductive polymer to react and bond with the organic acid to obtain an organic acid grafted onto the ion-conductive polymer; wherein the molar ratio of the organic acid to the ion-conductive polymer is 1:(0.5-2); (4) The composite material S2 is subjected to polymerization reaction with an electronic conductive polymer monomer and an organic acid grafted with an ion conductive polymer in the presence of an oxidant, wherein the mass ratio of the composite material S2 to the electronic conductive polymer monomer is 1:(0.05-0.2), and the molar ratio of the electronic conductive polymer monomer, the organic acid grafted with the ion conductive polymer and the oxidant is 1:(0.5-2):1; after filtering and drying, a composite material coated with a mixed conductor membrane is obtained, i.e., a negative electrode material, wherein the cross-linked mixed conductor membrane material is uniformly coated on the surface of the composite material particles.

2. The negative electrode material for lithium-ion batteries according to claim 1, It is characterized in that The ion conductive polymer is selected from one of polyethylene oxide, polyethylene glycol, polyethylene glycol diglycidyl ether, polyacrylonitrile, and lithiated polyacrylic acid; the electron conductive polymer is selected from one of polyaniline, polypyrrole, and poly(ethylenedioxythiophene).

3. The method for preparing the negative electrode material for a lithium ion battery according to claim 1 or 2, It is characterized in that The following steps are involved: (1) If the negative electrode particles are porous silicon or nano silicon, they are first carbon coated to form micron particles, wherein the carbon coating method is to mix the negative electrode particles with a carbon source, and to coat the carbon source by a chemical method, wherein the mass ratio of the carbon source to the negative electrode particles is 1:(1-9); and then carbonized in an inert atmosphere; if the negative electrode particles are micron silicon or silicon oxide, this step is not required; Material S1 is obtained through the above steps; (2) The material S1 is surface modified by using a surface modifier, so that the comonomer compound of the electronic conductive polymer is grafted onto the surface of the material to obtain the composite material S2; the surface modification method is: a silane coupling agent, material S1 and a solvent are mixed, and the reaction is carried out at 80°C for 2 hours to graft the active group onto the silicon surface, wherein the mass ratio of the material S1 to the silane coupling agent is 1:(0.01-0.02), and the solvent is a mixed solvent of water and ethanol; then the reaction product is mixed with the comonomer compound of the electronic conductive polymer and a solvent for reaction, wherein the solvent is a mixed solvent of water and ethanol, wherein the molar ratio of the silane coupling agent to the comonomer compound of the electronic conductive polymer is (0.8-1.2):1, the reaction temperature is 80°C-120°C, and the reaction time is 3-8 hours; (3) Using an organic acid with multiple functional groups as a crosslinking center to induce the terminal functional groups of the ion-conductive polymer to react and bond with the organic acid to obtain an organic acid grafted onto the ion-conductive polymer; wherein the molar ratio of the organic acid to the ion-conductive polymer is 1:(0.5-2); (4) The composite material S2 is subjected to polymerization reaction with an electronic conductive polymer monomer and an organic acid grafted with an ion conductive polymer in the presence of an oxidant, wherein the mass ratio of the composite material S2 to the electronic conductive polymer monomer is 1:(0.05-0.2), and the molar ratio of the electronic conductive polymer monomer, the organic acid grafted with the ion conductive polymer and the oxidant is 1:(0.5-2):1; after filtering and drying, a composite material coated with a mixed conductor membrane is obtained, i.e., a negative electrode material, wherein the cross-linked mixed conductor membrane material is uniformly coated on the surface of the composite material particles.

4. The preparation method according to claim 3, It is characterized in that The carbon source in step (1) is selected from at least one of asphalt, phenolic resin, polyvinyl chloride, glucose and citric acid.

5. The preparation method according to claim 3, It is characterized in that The chemical method of step (1) is spray drying or rotary evaporation; the carbonization temperature is 600-900°C, and the carbonization heating rate is 5-10°C / min; the inert atmosphere is argon, or a mixture of argon and hydrogen, or a mixture of nitrogen and hydrogen.

6. The preparation method according to claim 3, It is characterized in that The silane coupling agent is selected from at least one of vinyl triethoxysilane, vinyl trimethoxysilane, and vinyl tri(β-methoxyethoxy)silane; the comonomer compound of the electronic conductive polymer is selected from at least one of m-phenylenediamine, p-phenylenediamine, triphenylamine, 2-pyrrolcarboxylic acid, and 3-pyrrolcarboxaldehyde.

7. The preparation method according to claim 3, It is characterized in that In step (3), the ion conductive polymer is selected from one of polyethylene oxide, polyethylene glycol, polyethylene glycol diglycidyl ether, polyacrylonitrile, and lithiated polyacrylic acid; the organic acid is selected from at least one of phytic acid, camphorsulfonic acid, and tannic acid; and the ion conductive polymer and the organic acid are stirred and reacted at a temperature of 120 to 150° C. for 2 to 4 hours to obtain an ion conductive polymer grafted with an organic acid.

8. The preparation method according to claim 3, It is characterized in that In step (4), the electronic conductive polymer monomer is selected from one of aniline, pyrrole, and poly (3,4-diethylenedioxythiophene); the selected oxidant is ammonium persulfate; in step (4), the oxidant solution is slowly added to a mixed solution of the composite material S2 powder, the electronic conductive polymer monomer, and the ion conductive polymer grafted organic acid.

9. Use of the lithium ion battery negative electrode material according to claim 1 in lithium ion batteries.