A high-foam-stable concrete air-entraining agent and its preparation method and application
By using a positively charged silicone coupling agent and tetraethyl orthosilicate and anionic air-entraining surfactant to encapsulate the air-entraining agent with a hollow spherical structure, the problems of easy precipitation and low encapsulation efficiency of traditional air-entraining agents are solved. , achieving improved stability and durability of concrete and a sustained-release effect of air-entraining agents.
Patent Information
- Application Number
- CN202211290422.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-10-21
AI Technical Summary
Traditional concrete air-entraining agents are easily chelated with salt ions to form precipitation or are embedded in hydration products, causing fluctuations in the air content of concrete and affecting durability. The existing packaging technology has low packaging efficiency, causing the air-entraining agent to be released too quickly.
Using a positively charged silicone coupling agent and tetraethyl orthosilicate as the silicon precursor, combined with an anionic air-entraining surfactant as a template agent, a highly stable foam-entraining air-entraining agent with a hollow sphere structure is formed through one-step encapsulation. , utilizing the adsorption, desorption and ion exchange of silica to achieve sustained release.
It improves the stability and durability of concrete, reduces the fluctuation of air content over time, delays the release of air-entraining agents, optimizes the bubble structure, and enhances the strength after hardening.
Smart Images

Figure CN117945685B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a high-foam-stable concrete air-entraining agent and a preparation method and application thereof. Background Art
[0002] With the vigorous development of infrastructure construction in my country, people are paying more and more attention to the durability of concrete. Adding air-entraining agent during concrete mixing can affect the bubble structure after coagulation and hardening, and then directly affect the concrete's anti-freeze-thaw, anti-medium penetration and structural stability. Traditional concrete air-entraining agent is a kind of amphiphilic surfactant molecule with a hydrophobic group at one end and a hydrophilic group at the other end. Traditional air-entraining agent is easy to chelate with salt ions to form precipitation or adsorb on the surface of cementitious materials and be embedded in hydration products, thereby reducing the concentration in the slurry solution, resulting in the time-dependent fluctuation of the air content of concrete and the deterioration of the bubble structure, thereby affecting the workability and durability of concrete. At present, domestic researchers generally use a variety of air-entraining and foam-stabilizing surfactants to improve the adaptability of the product, but this method may produce precipitation due to the instability of multiple components, and will also affect the fluidity and strength of concrete. There is also an improvement in the traditional structure of surfactants to overcome the disadvantages of traditional air-entraining agents, but its synthesis method is relatively complicated, and the residual chemical components will affect the durability of the material.
[0003] Sustained-release technology is an important means to improve the time-dependent behavior of materials, and is currently widely used in the fields of medicine and oil fields. Patent KR101903000B1 uses an emulsion template method to prepare core-shell insect repellent nanopowder using cationic surfactants and anionic silica precursors. However, this emulsion method requires the preparation of two phases of oil and water, which are hydrolyzed at the interface to form a hollow structure. The operation is relatively difficult, which affects the later industrial application.
[0004] Patent CN104548105B uses surfactant micelles that solubilize hydrophobic substances as templates and adopts a one-step method to directly prepare hollow silica microcapsules that encapsulate hydrophobic substances. This solution uses the solubilization of hydrophobic substances by surfactants to carry hydrophobic substances into the interior of silica, and is suitable for some hydrophobic substances.
[0005] Patent CN103011182B uses sodium dodecyl sulfate and hexadecyltrimethylammonium bromide as templates, and obtains vesicular mesoporous silica as a sustained-release material through steps such as hydrolysis, hydrothermal treatment, and calcination. This material subsequently needs to be impregnated for a long time to encapsulate the guest material, but the encapsulation efficiency is not high, resulting in a faster release of the guest material in the early stage. Summary of the invention
[0006] In order to solve the problems in the prior art that the traditional air-entraining components in the prior art are easily chelated with salt ions to form precipitation or adsorbed on the surface of cementitious materials and embedded in hydration products, resulting in the failure of the air-entraining components, and the traditional encapsulation technology is achieved by long-term immersion and the encapsulation efficiency is not high. The present application provides a high-foam-stable concrete air-entraining agent and its preparation method and application, using positively charged silicon-oxygen coupling agent and tetraethyl orthosilicate as silicon precursors, anionic air-entraining surfactants as templates, and the positively charged groups provide an anchoring effect for the interaction with negatively charged surfactant molecules, and the anionic air-entraining surfactants are encapsulated in the interior of silica to form a high-foam-stable air-entraining agent with a hollow sphere structure.
[0007] A high-stable foam type air-entraining agent for concrete, which is obtained by mixing a silicon precursor and a template agent, heating and hydrolyzing them; the silicon precursor comprises a silane coupling agent and tetraethyl orthosilicate, and the silane coupling agent is positively charged; the template agent is an anionic air-entraining surfactant; the mass ratio of the tetraethyl orthosilicate, the silane coupling agent and the anionic air-entraining surfactant is 1:(0.4-0.6):(0.5-3.0); and the particle size of the high-stable foam type air-entraining agent is 100-300nm.
[0008] By changing the raw material ratio to control the particle size of the high-stable foaming air-entraining agent and the loading amount of the air-entraining agent component, a series of high-stable foaming air-entraining agents with hollow sphere structures having a particle size of 100-300nm and an air-entraining component loading amount greater than 15% are obtained. The air-entraining agent molecules are controlled to escape at a certain speed, thereby compensating for the air-entraining agent content lost due to the influence of the cement environment and reducing the time fluctuation of the air content of the concrete.
[0009] The silane coupling agent is at least one of positively charged silane coupling agents such as γ-aminopropyltriethoxysilane (KH550), N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane (KH792), and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane (KH602).
[0010] The anionic air-entraining surfactant is at least one of anionic surfactants such as sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium dodecyl polyoxyethylene ether sulfate, and sodium α-olefin sulfonate.
[0011] Positively charged siloxane coupling agent and tetraethyl orthosilicate are used as silicon precursors, and anionic air-entraining surfactant is selected as template. The positively charged group provides an anchoring effect for interaction with negatively charged surfactant molecules, and the anionic air-entraining surfactant is encapsulated inside to form a high-stable foam-entraining agent with a hollow sphere structure. The high-stable foam-entraining agent is directly added to concrete. Initially, a part of the air-entraining component is released due to the adsorption and desorption effect on the surface of silica. Later, after ion exchange and alkaline etching in the cement environment, the air-entraining component encapsulated by silica is slowly released to make up for the air-entraining agent content lost due to the influence of the cement environment. At the same time, the silica itself has undergone a certain degree of hydrophobic modification, which has a good effect of optimizing the bubble structure, and can also promote hydration reaction and improve the strength after hardening.
[0012] A method for preparing a high-stable foaming air-entraining agent for concrete comprises the following steps: (1) dispersing tetraethyl orthosilicate and a siloxane coupling agent in anhydrous ethanol to obtain a silicon precursor dispersion; (2) dissolving an anionic air-entraining surfactant in water and ethanol, then heating the mixture to 70-80°C, stirring the mixture at a speed of 300-500 rpm, and slowly dripping the silicon precursor dispersion during the stirring process; (3) continuing the reaction for 2-8 hours after the dripping is completed, then aging the mixture at room temperature for 16-22 hours, and finally centrifuging, washing, and drying the mixture to obtain hollow silicon dioxide microspheres encapsulating the air-entraining surfactant, namely, the high-stable foaming air-entraining agent for concrete.
[0013] In the above step (1), the mass ratio of anhydrous ethanol to tetraethyl orthosilicate is (5-10):1; in the above step (2), the mass ratio of water, ethanol and tetraethyl orthosilicate in the silicon precursor dispersion is (80-110):(20-30):1.
[0014] The invention discloses an application of a high-stable foam type air entraining agent for concrete. The high-stable foam type air entraining agent for concrete is applied in a concrete construction process, and the dosage of the high-stable foam type air entraining agent for concrete is 0.002% to 0.02% of the mass of cementitious materials in concrete.
[0015] The high-stable foam-type air-entraining agent for concrete of the present invention is a powder and should be added to the concrete during concrete mixing and preparation. In order not to affect the slow-release effect, it should not be mixed with water in advance.
[0016] The high-stable foam-entraining agent of the present invention can also be obtained by mixing tetraethyl orthosilicate and a negatively charged silane coupling agent as a silicon precursor and a cationic air-entraining surfactant as a template, heating and hydrolyzing. The interaction between anions and cations also provides an anchoring effect for the formation of silica microspheres encapsulating the air-entraining surfactant.
[0017] Compared with the prior art, the present invention has the following advantages:
[0018] 1. The high-stable foam-entraining agent of the present invention uses positively charged siloxane coupling agent and tetraethyl orthosilicate as silicon precursors, selects anionic air-entraining surfactant as template, and the positively charged group provides an anchoring effect for interaction with negatively charged surfactant molecules. The anionic air-entraining surfactant is encapsulated into the interior to form a high-stable foam-entraining agent with a hollow sphere structure through a one-step method. This method is simple and provides a new feasible scheme for encapsulating anionic surfactants.
[0019] 2. The particle size of the highly stable foaming air-entraining agent is 100-300nm, and the thickness of the silica shell is 10-20nm. When directly added to concrete, a part of the air-entraining components are initially released due to the adsorption and desorption effect on the surface of silica. Later, through ion exchange and alkaline etching in the cement environment, the air-entraining components encapsulated by silica are slowly released to make up for the air-entraining agent content lost due to the influence of the cement environment. At the same time, the silica itself has undergone a certain degree of hydrophobic modification, which has a good effect of optimizing the bubble structure and can also promote hydration reaction, which can make up for the strength loss caused by the air content.
[0020] 3. The slow-release air-entraining material of the present invention has a simple preparation method, is easy to use and has low cost; it can effectively reduce the time-dependent fluctuation of the air content in cement-based materials, and can also improve the strength and durability of hardened concrete. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic diagram of the structure of the high-stable foam type air-entraining agent of this application;
[0022] Figure 2 is the SEM image of the high-stable foam type air-entraining agent of Example 1-3;
[0023] Figure 3 is a TEM image of the high-stable foam type air-entraining agent of Example 1;
[0024] Figure 4 is a sustained release curve of the high-stable foam type air-entraining agent of Example 1 in a Ca(OH)2 alkaline aqueous solution; DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] All materials used are commercially available products, among which all reagents (analytical grade) used for the preparation of high-foam-stable air-entraining agent for concrete based on SiO2 / air-entraining surfactant capsule coating materials were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., and the air-entraining agent, siloxane coupling agent and polycarboxylic acid water-reducing agent in the examples were from Jiangsu Subote New Materials Co., Ltd.
[0027] Example 1
[0028] 10 g of tetraethyl orthosilicate and 5 g of γ-aminopropyltriethoxysilane were dispersed in 30 g of anhydrous ethanol to obtain a silicon precursor dispersion;
[0029] 5g of sodium dodecyl sulfate was dissolved in 1000g of water and 70g of ethanol, then heated to 70°C, stirred at 400rpm, and the silicon precursor dispersion was slowly added dropwise during the stirring process. After the addition was completed, the reaction was continued for 6h, and then aged at room temperature for 18h. Finally, after centrifugation, washing, and drying, silica microspheres encapsulating sodium dodecyl sulfate were obtained, i.e., a high-stable foam-entraining agent. The organic matter loading was 35%, and the particle size was about 274nm. Figure 3 It shows that the prepared silica microspheres have a hollow structure.
[0030] Example 2
[0031] 10 g of tetraethyl orthosilicate and 4 g of N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane were dispersed in 30 g of anhydrous ethanol to obtain a silicon precursor dispersion;
[0032] 15g of sodium dodecyl sulfate was dissolved in 1000g of water and 70g of ethanol, then heated to 75°C, stirred at 450rpm, and the silicon precursor dispersion was slowly added dropwise during the stirring process. After the addition was completed, the reaction was continued for 4h, and then aged at room temperature for 20h. Finally, after centrifugation, washing, and drying, silica microspheres encapsulating sodium dodecyl sulfate were obtained, i.e., a high-stable foam-entraining agent. The organic matter loading was 31%, and the particle size was about 160nm.
[0033] Example 3
[0034] 10 g of tetraethyl orthosilicate and 4 g of N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane were dispersed in 30 g of anhydrous ethanol to obtain a silicon precursor dispersion;
[0035] 30g of sodium dodecyl sulfate was dissolved in 1000g of water and 70g of ethanol, then heated to 80°C, stirred at 500rpm, and slowly added with silicon precursor dispersion during stirring. After the addition was completed, the reaction was continued for 2h, and then aged at room temperature for 22h. Finally, after centrifugation, washing, and drying, silica microspheres encapsulating sodium dodecyl sulfate were obtained, i.e., high-stable foam-entraining agent. The organic matter loading was 29%, and the particle size was about 65nm.
[0036] Example 4
[0037] 10 g of tetraethyl orthosilicate and 4 g of γ-aminopropyltriethoxysilane were dispersed in 30 g of anhydrous ethanol to obtain a silicon precursor dispersion;
[0038] (2) 20 g of sodium dodecylbenzene sulfonate was dissolved in 1000 g of water and 80 g of ethanol, and then the temperature was raised to 70° C. and stirred at 500 rpm. During the stirring process, the silicon precursor dispersion was slowly added dropwise. After the addition was completed, the reaction was continued for 6 h, and then aged at room temperature for 18 h. Finally, the silicon dioxide microspheres encapsulating sodium dodecylbenzene sulfonate were obtained by centrifugation, washing, and drying, i.e., a high-stable foam-type air-entraining agent. The organic matter loading was 28%, and the particle size was about 127 nm.
[0039] Example 5
[0040] 10 g of tetraethyl orthosilicate and 6 g of γ-aminopropyltriethoxysilane were dispersed in 20 g of anhydrous ethanol to obtain a silicon precursor dispersion;
[0041] 20g of sodium dodecyl polyoxyethylene ether sulfate was dissolved in 1000g of water and 60g of ethanol, then heated to 70°C, stirred at 450rpm, and slowly added with silicon precursor dispersion during stirring. After the addition was completed, the reaction was continued for 7h, and then aged at room temperature for 17h. Finally, after centrifugation, washing, and drying, silica microspheres encapsulating sodium dodecyl polyoxyethylene ether sulfate were obtained, i.e., a highly stable foaming air entraining agent. The organic matter loading was 32% and the particle size was about 134nm.
[0042] Comparative Example 1
[0043] 10g of tetraethyl orthosilicate and 5g of γ-aminopropyltriethoxysilane were dispersed in 30g of anhydrous ethanol to obtain a silicon precursor dispersion; 1000g of water and 70g of ethanol were placed in a flask, heated to 70°C, stirred at 400rpm, and the silicon precursor dispersion was slowly added dropwise during the stirring process. After the addition was completed, the reaction was continued for 6h, and then aged at room temperature for 18h. Finally, after centrifugation, washing, and drying, silicon dioxide microspheres modified with a silicon-oxygen coupling agent were obtained. The loading amount of organic matter was 13%, and the particle size was about 306nm.
[0044] Comparative Example 2
[0045] Sodium dodecyl sulfate was used as an air entraining agent.
[0046] Comparative Example 3
[0047] 10g of tetraethyl orthosilicate was dispersed in 30g of anhydrous ethanol to obtain a silicon precursor dispersion; 5g of sodium dodecyl sulfate was dissolved in 1000g of water and 70g of ethanol, then heated to 70°C, stirred at 400rpm, and the silicon precursor dispersion was slowly added dropwise during the stirring process. After the addition was completed, the reaction was continued for 6h, and then aged at room temperature for 18h. Finally, after centrifugation, washing, and drying, silica microspheres loaded with sodium dodecyl sulfate were obtained. The loading amount of organic matter was 8%, and the particle size was about 257nm.
[0048] Test Example 1: Test on the slow-release effect of high-stable foam-type air-entraining agent
[0049] The release effect of the prepared high-foam-stable concrete air-entraining agent was investigated by simulating cement paste with a Ca(OH)2 alkaline aqueous solution. The silica microspheres encapsulating sodium dodecyl sulfate prepared in Example 1 were dispersed in a Ca(OH)2 alkaline aqueous solution and stirred. The supernatant was taken at 5 min, 30 min, 60 min, 90 min, and 120 min, and the TOC test was performed to determine the air-entraining agent content released. Figure 4 As shown, the sample presents an ideal slow release rate within 2 hours. This indicates that the high-stable foam-type air-entraining agent obtained in the present application has a good slow release effect in concrete applications, releases a portion of the air-entraining component in the initial stage, has a certain air-entraining effect, and reduces the time-dependent fluctuation of the air content by continuously releasing the air-entraining component in the later stage.
[0050] Test Example 2: Test of air content and strength of concrete
[0051] The test was carried out in accordance with the relevant provisions of GB8076-2008 "Concrete Admixtures", and the application effect of the prepared high-stable foam air-entraining agent for concrete was examined through concrete tests. The silica microspheres encapsulating the air-entraining agent prepared in Examples 1-5 and the samples in Comparative Examples 1-3 were tested for concrete air content and strength, wherein the concrete mix ratios used are shown in Table 1:
[0052] Table 1
[0053] cement Sand Dashi Xiaoshi water Polycarboxylate water reducer / adhesive 6.60kg 14.6kg 14.3kg 9.5kg 2.65kg 0.18wt%
[0054] The cement used is Jiangnan Onoda P.II 52.5 cement, the fly ash is Class II fly ash, the sand is medium sand with a fineness modulus Mx=2.7, and the coarse aggregate is 5-20 mm continuously graded crushed stone. The polycarboxylic acid water reducer used is provided by Jiangsu Subote New Materials Co., Ltd. All samples are pre-mixed with cement. All embodiments and comparative examples 1 and 3 have the same dosage, which is 0.01% of the mass of the cementitious material in the concrete. The dosage of comparative example 2 is adjusted to the same initial air content as that of embodiment 1. The test results are shown in Table 2.
[0055] Table 2
[0056]
[0057] It can be seen from Table 2 that the air content loss of concrete with silica microspheres encapsulating air entraining agent is extremely low over time, and has ideal foam stabilization performance. At the same time, the strength of the test block at different ages is less reduced than that of the blank group; comparing the blank group and comparative example 1, it is found that the initial air content of the concrete with only silica added is slightly higher, and the compressive strength is higher than that of the blank group, indicating that the introduction of silica has a certain foam stabilization effect and is conducive to the improvement of strength after hardening; comparing Example 1 and Comparative Example 2, it is found that the concrete with silica microspheres encapsulating sodium dodecyl sulfate has a certain air entrainment effect initially, and the air content loss over time is very small compared with the experimental group with only sodium dodecyl sulfate, and the strength of the test block at different ages is less different. Comparing Example 1 and Comparative Example 3, it is found that there is no anchoring effect of the siloxane coupling agent, the loading amount of sodium dodecyl sulfate of the obtained silica is low, and the release is concentrated at the initial stage, without subsequent sustained release effect. It shows that the foam stabilizer based on inorganic capsule material of the present invention has good foam stabilizing performance while having a small reduction in concrete strength; by comparing Examples 1-3, it can be seen that the samples with smaller particle sizes have higher initial air content and higher loss over time because more air entraining agent is adsorbed and less air is encapsulated inside.
[0058] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high-foam-stable air-entraining agent for concrete. Features: The high-foam-stable air-entraining agent is obtained by mixing a silicon precursor and a template agent and heating and hydrolyzing them; The silicon precursor comprises a silane coupling agent and tetraethyl orthosilicate, and the silane coupling agent is positively charged; The silane coupling agent is at least one of γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane; The template agent is an anionic air-entraining surfactant; the anionic air-entraining surfactant is at least one of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, sodium dodecyl polyoxyethylene ether sulfate, and sodium α-olefin sulfonate; The mass ratio of tetraethyl orthosilicate, siloxane coupling agent and anionic air-entraining surfactant is 1:(0.4-0.6):(0.5-3.0); The preparation of the highly stable foaming air-entraining agent comprises the following steps: (1) dispersing tetraethyl orthosilicate and a siloxane coupling agent in anhydrous ethanol to obtain a silicon precursor dispersion; (2) dissolving an anionic air-entraining surfactant in water and ethanol, then heating to 70-80° C., stirring at a speed of 300-500 rpm, and slowly dropping the silicon precursor dispersion during the stirring process; (3) continuing the reaction for 2-8 hours after the dropwise addition is completed, then aging at room temperature for 16-22 hours, and finally centrifuging, washing, and drying to obtain hollow silica microspheres encapsulating the air-entraining surfactant, namely, a highly stable foaming air-entraining agent for concrete.
2. A high foam-stable concrete air-entraining agent according to claim 1, Features: The particle size of the high-stable foam type air-entraining agent is 100-300nm.
3. A high-foam-stable concrete air-entraining agent according to claim 1, Features: In the step (1), the mass ratio of anhydrous ethanol to tetraethyl orthosilicate is (5-10):
1.
4. A high-foam-stable concrete air-entraining agent according to claim 1, Features: In the step (2), the mass ratio of water, ethanol and tetraethyl orthosilicate in the silicon precursor dispersion is (80-110):(20-30):
1.
5. Application of a high-foam-stable air-entraining agent for concrete, Features: The high-stable foam type air-entraining agent for concrete is used in the concrete construction process, and the dosage of the high-stable foam type air-entraining agent for concrete is 0.002% to 0.02% of the mass of the cementitious material in the concrete; the high-stable foam type air-entraining agent for concrete is the high-stable foam type air-entraining agent for concrete described in claim 1.
Citation Information
Patent Citations
Synthesis method of vesicular mesoporous silicon dioxide
CN103011182B
Hollow silica microcapsules encapsulated with hydrophobic substances and preparation method thereof
CN104548105B
Antisect nano powder having core-shell shape capable of controlling release velocity and manufacturing method of the same
KR101903000B1
Slow-release air-entraining type nano-porous composite material as well as preparation method and application thereof
CN114685079A
Core-shell hybrid nano functional material as well as preparation method and application thereof
CN114685082A