A method for reducing wafer surface roughness
By using gases such as C4F8 in the plasma reaction chamber to form polymers and react with the tungsten surface, the problem of difficulty in reducing the roughness of the tungsten surface is solved, the wafer surface is flattened, and the device integration and reliability are improved .
Patent Information
- Application Number
- CN202410207687.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-02-26
AI Technical Summary
In the semiconductor wafer manufacturing process, the roughness of the tungsten surface is difficult to effectively reduce, which affects the integration and reliability of the device. The existing CMP process has limited effect in metal embolization between different conductive layers.
Using a process method of deposition and etching, the polymer is formed by using gases such as C4F8 in the plasma reaction chamber and adsorbing it on the tungsten surface to fill the recessed area, and at the same time, the F free radical reacts with tungsten to generate volatile by-products. The surface is flattened.
It effectively reduces the roughness of the wafer surface after tungsten CVD, improves the surface flatness, and improves the integration and reliability of the device.
Smart Images

Figure CN117976535B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of semiconductor wafer manufacturing, and in particular relates to a method for reducing the surface roughness of a wafer. Background Art
[0002] Tungsten is widely used in DRAM chips to form bit lines and bit line contact plugs. Tungsten or tungsten silicide can form DRAM word lines with polysilicon. As feature sizes continue to shrink, tungsten is used to form DRAM FEoL contact plugs. For buried word line (bwl) DRAM, tungsten is combined with titanium nitride to form word lines and gate electrodes of array transistors, and combined with polysilicon to form bit lines and gate electrodes of peripheral MOSFETs.
[0003] Therefore, the surface flattening of tungsten will further affect the integration, reliability and quality rate of the device. At present, the CMP (chemical mechanical polishing) process of tungsten is widely used in the formation of metal plugs between different conductive layers, because this flattening technology can improve the yield rate. Summary of the invention
[0004] The purpose of the present invention is to provide a method for reducing the surface roughness of a wafer, using a deposition and etching process to improve the surface roughness of a wafer after tungsten CVD. To achieve the above purpose, the technical solution adopted is as follows:
[0005] A method for reducing the surface roughness of a wafer comprises the following steps:
[0006] Step 1, place the wafer in the etching reaction chamber, and set the chamber pressure to 10mt-1000mt, the RF power range to 200W-1000W, and the base temperature to 50-300°C;
[0007] Step 2, introducing the main etching gas, C4F8 and the regulating gas into the plasma generating chamber, and the etching gas, C4F8 and the regulating gas respectively form plasma in the plasma generating chamber after passing through the radio frequency generator;
[0008] Among them, C4F8 forms a polymer after passing through a radio frequency generator, which is adsorbed on the tungsten surface and fills the concave area, thereby improving the surface flatness;
[0009] The main etching gas is decomposed by the RF generator to generate F radicals which react with tungsten to generate volatile by-products WFx to achieve etching.
[0010] Preferably, in step 2, the main etching gas is a mixed gas of NF3 and CF4; the regulating gas is a mixed gas of O2, He, N2 and Ar.
[0011] Preferably, the free radicals and ions in the plasma reach the surface of the gas homogenizing disk by diffusion, and after passing through the gas homogenizing disk, the ratio of the free radicals and ions entering the etching reaction chamber increases.
[0012] Preferably, the gas uniforming disk is detachably disposed in the plasma generating chamber and between the etching reaction chamber.
[0013] Compared with the prior art, the advantages of the present invention are:
[0014] 1. The process method of deposition (C4F8) and etching (main etching gas) is used to improve the roughness of the wafer surface after tungsten CVD.
[0015] 2. Improve the surface roughness of the sample by selecting gas type, gas flow, pressure range, and gas pass rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 is a structural diagram of a remote plasma device;
[0017] Figure 2 is the sample initial state diagram;
[0018] Figure 3 This is a schematic diagram of a sample with a roughness of 4.09 nm after treatment in Example 5. DETAILED DESCRIPTION
[0019] The method for reducing the surface roughness of a wafer of the present invention will be described in more detail below in conjunction with a schematic diagram, wherein a preferred embodiment of the present invention is shown, and it should be understood that those skilled in the art can modify the present invention described herein while still achieving the advantageous effects of the present invention. Therefore, the following description should be understood as being widely known to those skilled in the art, and not as a limitation of the present invention.
[0020] A method for reducing the surface roughness of a wafer comprises the following steps:
[0021] Step 1, place the wafer in the etching reaction chamber, and set the chamber pressure to 10mt-1000mt, the RF power range to 200W-1000W, and the base temperature to 50-300°C;
[0022] Step 2, introducing the main etching gas, C4F8 and the regulating gas into the plasma generating chamber, and the etching gas, C4F8 and the regulating gas respectively form plasma in the plasma generating chamber after passing through the radio frequency generator;
[0023] Among them, C4F8 forms a polymer with the main component of -CF2-CF2-CF2-CF2- after passing through the radio frequency generator, which is adsorbed on the tungsten surface and fills the recessed area, thereby improving the surface flatness.
[0024] Specifically, the induced electric field generated by the radio frequency current passing through the coil (ICP) can accelerate electrons to continuously collide with C4F8 molecules to decompose them and form polymers.
[0025] The main etching gas is decomposed by the RF generator to generate F radicals which react with tungsten to generate volatile by-products WFx to achieve etching.
[0026] The sample provided by the present invention has a W deposit height of 360 nm, a Ti height of 90 nm, a TiN height of 15 nm before etching, and an initial roughness Ra of 7.85 nm.
[0027] The present invention provides some embodiments to illustrate the improvement effect and action principle of different gas types, pressures, and gas passing rates on the surface roughness of samples.
[0028] The remote plasma device reaction chamber provided by the present invention is as follows Figure 1 As shown, it is mainly divided into two parts.
[0029] The upper part of the chamber is the plasma generation chamber (chamber 1), the lower part is the etching reaction chamber (chamber 2), and the middle part is the gas distribution disk, the diameter of the circular hole ranges from 1 to 5 mm, and the gas flow rate is 0.5% to 50%.
[0030] The reaction gas is introduced from the upper end of the chamber 1, and then the RF source generates plasma in the chamber 1 by inductive coupling through the surrounding coil (RF generator). The particles (free radicals and ions, etc.) in the plasma reach the surface of the gas-distributing disk by diffusion. At this time, some free radicals and ions in the plasma cannot enter the chamber 2 through the gas-distributing disk due to consumption effects such as collision and adsorption.
[0031] In addition, the concentration of free radicals in the plasma is much higher than the concentration of ions. After filtering by the gas-uniform disk, under the same consumption conditions, the ratio of free radicals to ions (the diameter of ions is larger than that of free radicals) entering the chamber 2 will further increase.
[0032] On the one hand, the free radicals entering the chamber 2 react chemically with the material to be etched (chemical etching) to generate volatile gas products which are pumped away by the vacuum system.
[0033] On the other hand, the number of ions entering the chamber 2 is reduced, resulting in a weakening of the bombardment effect (physical etching) on the material surface, so the proportion of chemical etching increases and the etching selectivity is higher.
[0034] The parameters of the remote plasma device are set as follows:
[0035] 1. The pressure range used in the process: 10mt-1000mt, the optimal choice is 50mt-600mt to achieve better etching effect. Too high or too low chamber pressure has a great impact on the reaction rate and etching uniformity.
[0036] 2. Process gas types and flow range:
[0037] Main etching gas: SF6, CF4, NF3 are the most commonly used gases for W etching. The F free radicals produced by decomposition can react with W to generate volatile by-product WF6.
[0038] The regulating or inhibiting gases include: single-component gases such as O2, Ar, N2, He, or mixed gases thereof.
[0039] C4F8 is the deposition gas.
[0040] The use range (flow rate) of reaction gas (SF6, CF4, NF3, C4F8) is: 10sccm-500sccm;
[0041] The gas used for regulation or suppression is in the range of 10sccm-500sccm.
[0042] 3. Base temperature control: The reaction temperature is 50-300℃. Under this process condition, the optimal choice of Base CF4 gas is 60-100℃. The reaction temperature of NF3, SF6, C4F8 is greater than 85℃, 85-120℃.
[0043] 4. RF parameter setting and usage range: Generally, a 13.56Mhz or 27Mhz RF generator is selected, and the usage range is 200W-1000W, with the optimal range being 400W-800W.
[0044] 5. Setting and use range of reaction time (etching time, calculated by the amount of tungsten etched in a certain period of time): According to the target roughness and etching depth of 270nm, the reaction time is calculated, generally 60s-180s, usually selected in 60s-100s.
[0045] Example 1
[0046] As shown in Table 1, it illustrates the effect of the gas distribution disk with different gas fluxes based on Recipe A on the surface roughness Ra of the sample.
[0047] When the gas flux is 10%, the surface roughness of the sample can be further reduced to 6.28 nm.
[0048] Using uniform gas plates with different gas fluxes (achieved by replacing uniform gas plates of different specifications) to adjust the concentration of free radicals and other particles in the reaction chamber can improve the etching selectivity and improve the surface roughness Ra of the sample.
[0049] Table 1
[0050]
[0051] Among them, the parameters of RecipeA are: chamber pressure, RF power, main etching gas flow rate, adjustment gas flow rate, base temperature, and reaction time.
[0052] In the following examples, the parameter explanations are similar to those in Example 1.
[0053] Example 2
[0054] As shown in Table 2, the effect of O2 and He addition on the surface roughness of the samples is explained.
[0055] Based on Recipe A, when the reaction gas contains O2 and He, the roughness of the sample can be reduced to 5.21nm.
[0056] The mechanism of action can be explained as the reaction of oxygen free radicals with W to form WOx products, and combined with the dilution effect of He, the surface after etching is smoother.
[0057] Table 2
[0058] Recipe Ra / nm initial 7.85 A:50mt / 500w / 50CF4 / 60N2 / 50NF3 / 50AR / 60℃ / 60s(base) 6.28 B:50mt / 500w / 50CF4 / 50NF3 / 100O2 / 60N2 / 50AR / 60℃ / 60s 5.35 C:50mt / 500w / 50CF4 / 50NF3 / 100He / 60N2 / 50AR / 60℃ / 60s 5.56 D:50mt / 500w / 50CF4 / 50NF3 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 5.21
[0059] Example 3
[0060] As shown in Table 3, the effect of adding SF6 at different flow rates based on Recipe D on the surface roughness of the sample is explained.
[0061] When the SF6 flow rate reaches 80sccm, the surface roughness of the sample can be further reduced to 4.22nm. Under the same gas flow, SF6 can produce more F (fluorine) radicals after dissociation. F-rich radicals can achieve better etching uniformity under certain pressure conditions.
[0062] Table 3
[0063] Recipe Ra / nm D:50mt / 500w / 50CF4 / 50NF3 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 5.21 E:50mt / 500w / 50CF4 / 50NF3 / 40SF6 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 4.45 F:50mt / 500w / 50CF4 / 50NF3 / 80SF6 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 4.22 G:50mt / 500w / 50CF4 / 50NF3 / 120SF6 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 5.23
[0064] Example 4
[0065] As shown in Table 4, the effect of adding C4F8 at different flow rates based on Recipe D on the surface roughness of the sample is illustrated.
[0066] When the flow rate of C4F8 reaches 40sccm, the surface roughness of the sample can be further reduced to 4.31nm. The main function of C4F8 is to form polymer. The main component of polymer is -CF2-CF2-CF2-CF2-polymer, which is adsorbed on the W surface and fills into the recessed area, thereby improving the surface flatness. At the same time, under the action of chemical etching, the surface roughness of the etched film becomes better.
[0067] Table 4
[0068] Recipe Ra / nm D:50mt / 500w / 50CF4 / 50NF3 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 5.21 H:50mt / 500w / 50CF4 / 50NF3 / 20C4F8 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 5.77 I:50mt / 500w / 50CF4 / 50NF3 / 30C4F8 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 5.23 J:50mt / 500w / 50CF4 / 50NF3 / 40C4F8 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 4.31 K:50mt / 500w / 50CF4 / 50NF3 / 50C4F8 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 4.45
[0069] Recipes H to K, the parameters are: chamber pressure, RF power, main etching gas flow rate, C4F8 flow rate, adjustment gas flow rate, base temperature, and reaction time.
[0070] Example 5
[0071] As shown in Table 5, it shows the effect of different pressures on the surface roughness of the sample based on Recipe J. When the process pressure is 200 mt, the surface roughness of the sample can be further reduced to 4.09 nm.
[0072] Table 5
[0073] Recipe Ra / nm J:50mt / 500w / 50CF4 / 50NF3 / 40C4F8 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 4.31 L:100mt / 500w / 50CF4 / 50NF3 / 40C4F8 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 4.24 M:150mt / 500w / 50CF4 / 50NF3 / 40C4F8 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 4.15 N:200mt / 500w / 50CF4 / 50NF3 / 40C4F8 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 4.09 O:300mt / 500w / 50CF4 / 50NF3 / 40C4F8 / 50O2 / 50He / 60N2 / 50AR / 60℃ / 60s 4.15
[0074] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any technician in the relevant technical field, without departing from the scope of the technical solution of the present invention, makes any form of equivalent replacement or modification to the technical solution and technical content disclosed in the present invention, which does not depart from the content of the technical solution of the present invention and still falls within the protection scope of the present invention.
Claims
1. A method for reducing the surface roughness of a wafer, characterized in that: The following steps are involved: Step 1, place the wafer in the etching reaction chamber, and set the chamber pressure to 10mt-1000mt, the RF power range to 200W-1000W, and the base temperature to 50-300°C; Step 2, introducing the main etching gas, C4F8 and the regulating gas into the plasma generating chamber, and the etching gas, C4F8 and the regulating gas respectively form plasma in the plasma generating chamber after passing through the radio frequency generator; Among them, C4F8 forms a polymer after passing through the radio frequency generator, which is adsorbed on the tungsten surface and fills the concave area, thereby improving the surface flatness; The main etching gas is a mixed gas of NF3 and CF4; the regulating gas is a mixed gas of O2, He, N2 and Ar; The main etching gas is decomposed by the radio frequency generator to generate F radicals which react with tungsten to generate volatile by-products to achieve etching.
2. The method for reducing wafer surface roughness according to claim 1, characterized in that: The free radicals and ions in the plasma reach the surface of the gas distribution disk by diffusion. After passing through the gas distribution disk, the proportion of free radicals and ions entering the etching reaction chamber increases.
3. The method for reducing wafer surface roughness according to claim 2, characterized in that: The gas uniforming disk is detachably arranged in the plasma generating chamber and between the etching reaction chamber.