A CO2 multi-level porous nanotube molecular sieve adsorbent and preparation method thereof

By preparing ZSM-5 molecular sieves co-modified with framework metals and heteronuclear metal oxide ultrafine nanoclusters, the problems of temperature sensitivity and low adsorption capacity of zeolite molecular sieves were solved, achieving high efficiency of CO2 adsorption performance and temperature adaptability, making it a suitable multi-level porous nanotube molecular sieve adsorbent for CO2.

CN117983194BActive Publication Date: 2024-11-05CHINESE RES ACAD OF ENVIRONMENTAL SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410212983.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-27
Publication Date
2024-11-05
Estimated Expiration
2044-02-27

AI Technical Summary

Technical Problem

Existing zeolite molecular sieves are sensitive to temperature changes, have low adsorption capacity, and their CO2 adsorption capacity decreases at high temperatures, making it difficult to meet the needs of carbon capture.

Method used

ZSM-5 molecular sieves co-modified with framework metals and heteronuclear metal oxide ultrafine nanoclusters were prepared by adopting a heteronuclear in-situ anchoring substitution mechanism and a two-step nucleation synergistic one-step dry gel crystallization method to form a hierarchical porous nanotube structure. Combined with carbon nanotubes and carbon fiber templates, a hierarchical porous nanotube molecular sieve adsorbent was prepared.

Benefits of technology

This improved the CO2 adsorption capacity and temperature adaptability of zeolite molecular sieves, enhanced the specific surface area and gas diffusivity of the adsorbent, and increased the adsorption efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a CO2 multi-level pore nanotube molecular sieve adsorbent and a preparation method thereof. Based on a heteronuclear in-situ anchoring substitution mechanism, a two-step nucleation coordinated one-step dry gel crystallization method is adopted to in-situ prepare a ZSM-5 molecular sieve co-modified with a skeleton metal and a heteronuclear metal oxide ultrafine nanocluster, wherein the skeleton metal ion radius is higher than the ion radius of the heteronuclear metal oxide; the skeleton metal is uniformly dispersed on the ZSM-5 skeleton, the heteronuclear metal oxide ultrafine nanocluster is highly dispersed on the ZSM-5 surface, and more active sites such as oxygen vacancies and acid sites are exposed on the surface of the ZSM-5 matrix; the invention adopts template agents such as carbon nanotubes and carbon fibers, and combines soft template agents such as polyquaternary ammonium salts to prepare a multi-level pore nanotube structure molecular sieve, the adsorbent has high specific surface area, developed pores, good gas diffusivity, is conducive to the exposure of active sites, and improves adsorption capacity and adsorption efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adsorbents, and in particular to a CO2 multi-level porous nanotube molecular sieve adsorbent and a preparation method thereof. Background Art

[0002] As the main greenhouse gas, CO2 is currently mainly removed by capture and storage technology. For the deep removal of low-content CO2, there are usually membrane separation, conversion and adsorption methods. The adsorption method has the advantages of high removal accuracy, no pollution to the environment, simple operation and low cost. The materials used for CO2 adsorption are mainly activated carbon, zeolite molecular sieves, metal oxides and metal organic framework materials (MOFs). Both activated carbon and zeolite molecular sieves use the advantages of their own developed pore structure and specific surface area to adsorb the adsorbate through van der Waals force or weak chemical bonds. Among them, zeolite molecular sieves have the advantages of large specific surface area, different structures and pores, and adjustable pore size. They are widely used as matrix materials for CO2 solid adsorbents. However, the biggest problem facing zeolite molecular sieves is that they are very sensitive to temperature changes. They only show ideal adsorption performance for CO2 at room temperature or even lower temperature conditions (far lower than the combustion flue gas temperature). When the temperature rises, its CO2 adsorption capacity will gradually decrease. In addition, the adsorption capacity is relatively low, and the adsorption process often requires a large amount of adsorption materials. If these problems can be effectively solved, zeolite materials will truly be feasible for capturing CO2.

[0003] Therefore, how to better improve the adsorption performance of zeolite molecular sieves, increase adsorption capacity, and improve temperature adaptability is an important issue that needs to be solved at present. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a CO2 multi-level porous nanotube molecular sieve adsorbent and a preparation method thereof. The high CO2 adsorption capacity zeolite molecular sieve designed and developed in this patent has good temperature adaptability and water resistance, and can better meet the current needs of carbon capture.

[0005] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is:

[0006] In a first aspect, a method for preparing a CO2 multi-level porous nanotube molecular sieve adsorbent is provided, which comprises the following steps:

[0007] S1: using sodium hydroxide, tetrapropylammonium hydroxide or tetrapropylammonium bromide, a mixed solution of silicon component, aluminum component, ammonia water, polyquaternary ammonium salt, and transition metal salt as raw materials, preparing an M-ZSM-5 crystal nucleus solution A having a skeleton lattice metal;

[0008] S2: adding heteronuclear metal N to the M-ZSM-5 crystal nucleus solution A, and nucleating under a certain pressure and temperature to prepare a crystal nucleus solution B of N-ZSM-5 with dispersed loading of surface metal M;

[0009] S3: Add a certain amount of carbon nanofibers and carbon nanotube templates impregnated with organic amine and silane, ethylenediaminetetraacetic acid, hexadecyltrimethylammonium bromide, and polyquaternary ammonium salt solvent to the above-mentioned crystal nucleus solution B, stir and dry gel, transfer to a polytetrafluoroethylene reactor, crystallize under a certain pressure and temperature, and obtain ZSM-5 nanotubes co-modified with skeleton lattice metal N and extra-skeleton ultrafine nanoclusters MOx on the inner and outer surfaces after three-stage calcination; immerse the obtained ZSM-5 nanotubes in an organic amine or silane solvent, and obtain a CO2 multi-level porous nanotube molecular sieve adsorbent after drying;

[0010] Among them, M represents a transition metal element, N represents a transition metal or a rare earth metal element, N-ZSM-5 is a multi-level porous nanotube molecular sieve with an MFI structure, the MOx ultrafine nanocluster is an ultrafine nanocluster oxide of metal M in a highly dispersed state, and N is a metal element whose metal ion radius is higher than that of M.

[0011] In a second aspect, an adsorbent is provided, which is a single-shell adsorbent with a general formula of U @ MOx ultrafine nanoclusters / N-ZSM-5 @ Y nanotubes, wherein M represents a transition metal element, N represents a transition metal or a rare earth metal element, and U and Y represent organic amines or silanes; the adsorbent is an integral nanotube molecular sieve adsorbent co-modified with MOx ultrafine nanoclusters and skeleton metal N inside and outside, wherein the MOx ultrafine nanoclusters are adjacent to the skeleton metal N and are highly dispersed on the surface of the ZSM-5 matrix, and interact and tightly bind with the ZSM-5 matrix; in addition, there is an organic film composed of organic amines or silanes on the inner and outer surfaces of the adsorbent, respectively.

[0012] In a third aspect, an adsorbent is provided, which is a double-shell adsorbent, and its general formula is U @ MOx ultrafine nanoclusters / N-ZSM-5@ROx ultrafine nanoclusters / P-ZSM-5 @ Y nanotubes, wherein M and R represent transition metal elements, N and P represent transition metals or rare earth metal elements, U and Y represent organic amines or silanes, N-ZSM-5 and P-ZSM-5 are multi-level porous molecular sieves with MFI structure, MOx and ROx ultrafine nanoclusters are ultrafine nanocluster oxides of transition metals, which are in a highly dispersed state, and N and P are metal elements whose metal ion radii are respectively higher than M and R; the inner layer of the adsorbent is an integral ZSM-5 multi-level porous nanotube co-modified with MOx ultrafine nanoclusters and skeleton metal N inside and outside, and MOx ultrafine nanoclusters are co-modified with MOx ultrafine nanoclusters and skeleton metal N inside and outside. The fine nanoclusters are close to the skeleton metal N and are highly dispersed on the surface of the ZSM-5 matrix, and interact and bind tightly with the ZSM-5 matrix; the outer layer is an integral ZSM-5 multi-level pore co-modified with ROx ultrafine nanoclusters and skeleton metal P inside and outside, the ROx ultrafine nanoclusters are close to the skeleton metal P and are highly dispersed on the surface of the ZSM-5 matrix, and interact and bind tightly with the ZSM-5 matrix; the inner and outer layers have a strong interaction and are tightly combined into an integral catalyst and adsorbent; there is an organic film composed of organic amine or silane on the inner and outer surfaces of the adsorbent respectively.

[0013] The beneficial effects of the present invention are:

[0014] 1. The present invention is based on the heteronuclear in-situ anchoring substitution mechanism, adopts a two-step nucleation coordinated one-step dry colloid crystallization method, and in-situ prepares a ZSM-5 molecular sieve co-modified with a framework metal and heteronuclear metal oxide ultrafine nanoclusters, wherein the framework metal ion radius is higher than the ion radius of the heteronuclear metal oxide; the framework metal is uniformly dispersed on the ZSM-5 framework, and the heteronuclear metal oxide ultrafine nanoclusters are highly dispersed on the ZSM-5 surface, and more active sites such as oxygen vacancies and acidic sites are exposed on the surface of the ZSM-5 matrix;

[0015] 2. The adsorbent developed by the present invention is ZSM-5, which is a multi-level pore nanotube molecular sieve. Template agents such as carbon nanotubes and carbon fibers are used, but are not limited to hard template agents, and also include carbon fibers synthesized hydrothermally by high polymer soft template agents, and combined with soft template agents such as polyquaternary ammonium salts to prepare multi-level pore nanotube structure molecular sieves. The adsorbent has a high specific surface area, developed pores, and good gas diffusion, which is conducive to the exposure of active sites and improves adsorption capacity and adsorption efficiency. DETAILED DESCRIPTION

[0016] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.

[0017] Example 1

[0018] An adsorbent is a single-shell adsorbent, and its general formula is U @ MOx ultrafine nanocluster / N-ZSM-5@ Y nanotube, wherein M represents a transition metal element, N represents a transition metal or a rare earth metal element, and U and Y represent organic amines or silanes. U @ MOx ultrafine nanocluster / N-ZSM-5 @ Y nanotube is a monolithic adsorbent, N-ZSM-5 is a multi-level porous nanotube molecular sieve with an MFI structure, MOx ultrafine nanocluster is an ultrafine nanocluster oxide of metal M (M=Mn, Ti, Fe, Ni and other transition metals), which is in a highly dispersed state; N is a metal element with a metal ion radius higher than M, and can be selected specifically according to the metal element M, wherein the selection range of N is transition metals such as Cu, Cr, Co or rare earth metal elements such as La and Ce, and U and Y represent organic amines or silanes.

[0019] The adsorbent is an integral nanotube molecular sieve adsorbent co-modified with MOx ultrafine nanoclusters and skeleton metal N inside and outside. The MOx ultrafine nanoclusters are adjacent to the skeleton metal N, highly dispersed on the surface of the ZSM-5 matrix, and tightly bound to the ZSM-5 matrix through interaction. In addition, there is an organic film composed of organic amine or silane on the inner and outer surfaces of the adsorbent, which has a certain hydrophobicity.

[0020] The preparation method comprises the following steps:

[0021] S1: Preparation of framework lattice metal M-ZSM-5 nucleus solution A

[0022] S101: mixing a soluble salt of transition metal M and deionized water in a certain proportion, and then adding a certain amount of tetrapropylammonium hydroxide or tetrapropylammonium bromide (TPAOH / TPABr) after thermal radiation combined with ultrasound and magnetic stirring, and then again thermal radiation combined with ultrasound and magnetic stirring to obtain a mixture a;

[0023] S102: A certain amount of sodium hydroxide is dissolved in deionized water, and a certain amount of aluminum component is added, after thermal radiation combined with ultrasound and magnetic stirring, a certain amount of silicon component is added, and thermal radiation combined with ultrasound and magnetic stirring for a certain period of time to obtain a mixture b;

[0024] S103: slowly pouring mixture a into mixture b, while maintaining thermal radiation stirring and ultrasonic oscillation for a certain period of time, to obtain mixture c;

[0025] S104: The mixture c is transferred to a polytetrafluoroethylene reactor, and nucleated for a certain period of time under a certain pressure and thermal radiation combined with microwave-assisted heating to obtain an M-ZSM-5 crystal nucleus solution A.

[0026] S2: Preparation of N-ZSM-5 crystal nucleus solution B with surface metal M dispersed load

[0027] S201: adding a certain amount of heteronuclear metal N soluble salt to the crystal nucleus solution A, and obtaining a mixture d after thermal radiation combined with ultrasound and magnetic stirring;

[0028] S202: Transfer the mixture d to a polytetrafluoroethylene reactor, and nucleate for a certain period of time under a certain pressure and thermal radiation combined with microwave-assisted heating to obtain a crystal nucleus solution B of N-ZSM-5 with dispersed surface metal M load.

[0029] S3: CO2 nanotube multi-level porous adsorbent co-modified with MOx ultrafine nanoclusters and skeleton metal N inner and outer surfaces

[0030] S301: Immerse a certain amount of carbon nanofibers, carbon nanotubes and other template agents in an organic amine or silane solvent of a certain concentration, filter and dry after immersing for a certain period of time.

[0031] S302: adding the dried product obtained in S301 to the crystal nucleus solution B, and obtaining a mixture f after thermal radiation combined with ultrasound and magnetic stirring;

[0032] S303: adding a certain amount of ethylenediaminetetraacetic acid (EDTA), cetyltrimethylammonium bromide (CTAB), polyquaternium salt and other solvents to the mixture f, and obtaining a mixture g after thermal radiation combined with ultrasound and magnetic stirring;

[0033] S304: After the mixture is dried by ultrasonic combined heating until it becomes a dry gel, it is transferred to a polytetrafluoroethylene reactor, crystallized for a certain period of time under a certain pressure and temperature, and calcined to obtain ZSM-5 multi-level porous nanotubes with inner and outer surfaces co-modified with skeleton lattice metal N and extra-skeleton ultrafine nanoclusters MOx, wherein M represents a transition metal element and N represents a transition metal or a rare earth metal element.

[0034] S305: The ZSM-5 multi-level porous nanotube adsorbent obtained in S304 is immersed in an organic amine or silane solvent of a certain concentration, and after being immersed for a certain period of time, filtered and dried to obtain a CO2 multi-level porous nanotube molecular sieve adsorbent.

[0035] Preferably, the soluble salt of the transition metal M in step S101 may be a soluble salt such as nitrates, chlorides, organic salts, etc. of transition metals such as Mn, Ti, Fe, Ni, etc., or may be one or a combination of different soluble salts.

[0036] Preferably, the aluminum component in step S102 can be one or more of aluminum-containing substances such as aluminum chloride, sodium aluminate, aluminum hydroxide, and aluminum triethanolate.

[0037] Preferably, the molar ratio of each component in the mixture c of steps S103 and S104 is:

[0038] SiO2:TPAOH or TPABr = 100:(10-35);

[0039] SiO2:H2O=100: (1000-8000);

[0040] SiO2:Na2O=100:(10-30);

[0041] SiO2:M=100:(0.05-3);

[0042] SiO2:Al2O3=100:(10-600);

[0043] Preferably, the heteronuclear metal N soluble salt in step S201 may be soluble salts such as organic salts, nitrates, chlorides, etc. of transition metals such as Cu, Cr, Co, or rare earth metal elements such as La, Ce, or may be one or a combination of different soluble salts.

[0044] Preferably, the molar ratio of heteronuclear metal N to silicon component in the mixture d of step S202 is:

[0045] SiO2:N=100:(0.05-3);

[0046] Preferably, in step S301, the solid-liquid ratio of the carbon nanofiber, carbon nanotube or other template agent to the organic amine or silane solution is 10:1, wherein the mass concentration of the organic amine or silane solution is 5-20%, and the drying temperature is 80-120°C;

[0047] Preferably, the organic amine or silane in step S301 is a solvent such as polyethyleneimine, phenylethylamine, trimethylchlorosilane, etc.;

[0048] Preferably, in step S302, the mass ratio of the amount of the template agent such as carbon nanofibers and carbon nanotubes added to the SiO2 in the mixture is (0.5-1.5):1;

[0049] Preferably, in step S303, the mass ratio of the added amount of solvents such as ethylenediaminetetraacetic acid (EDTA), cetyltrimethylammonium bromide (CTAB), and polyquaternium salt to the mass ratio of SiO2 in the mixture is (0.05-0.8):1;

[0050] Preferably, the polyquaternary ammonium salt in step S303 can be polypropylene dimethyl ammonium chloride, polyacrylamide, N-vinyl pyrrolidone and quaternized vinyl imidazole copolymer, etc.

[0051] Preferably, during the crystallization process in step S304, a small amount of deionized water is added to the reactor, the mass ratio of the added water to the dry glue is (0.5-2):1, the crystallization temperature is 140-200°C, and the crystallization time is 24-48h.

[0052] Preferably, the calcination process of step S304 in air atmosphere is divided into three stages: in the first stage, the crystallized product is dried at 100-120°C for 2-3h; in the second stage, the temperature is slowly increased from 100-120°C to 300-400°C at a heating rate of 1-5°C, and kept constant for 3-5h; in the third stage, the calcination temperature is slowly increased to 500-700°C at a heating rate of 1-5°C, and kept constant for 4-6h.

[0053] Preferably, the solid-liquid ratio of the impregnation in step S305 is 10:1, wherein the mass concentration of the organic amine or silane solution is 5-20%, the drying temperature is 80-120° C., and the organic amine or silane is a solvent such as polyethyleneimine, phenylethylamine, trimethylchlorosilane, etc.;

[0054] Preferably, in steps S1, S2 and S3, the ultrasonic power is 50-300 W, the heating temperature is 50-80° C., the magnetic stirring speed is 400-800 r / min, and the ultrasonic combined with thermal radiation magnetic stirring time is 60-120 min;

[0055] Preferably, the nucleation in steps S1 and S2 is carried out in a sealed reactor, the nucleation temperature is 80-120° C., the pressure is adjusted according to the temperature, the microwave power is 300-600 W, and the nucleation time is 8-20 h;

[0056] Example 2

[0057] An adsorbent is a double-shell adsorbent, and its general formula is U@MOx ultrafine nanoclusters / N-ZSM-5@ROx ultrafine nanoclusters / P-ZSM-5@Y nanotubes, wherein M and R represent transition metal elements, N and P represent transition metals or rare earth metal elements, and U and Y represent organic amines or silanes.

[0058] Among them, U@MOx ultrafine nanoclusters / N-ZSM-5@ROx ultrafine nanoclusters / P-ZSM-5@Y nanotubes are integral adsorbents, N-ZSM-5 and P-ZSM-5 are multi-level porous molecular sieves with MFI structure, MOx and ROx ultrafine nanoclusters are ultrafine nanocluster oxides of transition metals such as Mn, Ti, Fe, and Ni, and are highly dispersed; N and P are metal elements whose metal ion radii are higher than M and R, respectively, and can be selected specifically according to the M and R metal elements, among which the selection range of N and P is transition metals such as Cu, Cr, and Co or rare earth metal elements such as La and Ce, and U and Y represent organic amines or silanes. The double-shell integral CO2 hierarchical nanotube adsorbent is co-modified with single-atom metal and heteronuclear metal oxide ultrafine nanoclusters inside and outside, wherein the inner layer is an integral ZSM-5 hierarchical nanotube co-modified with MOx ultrafine nanoclusters and skeleton metal N inside and outside, the MOx ultrafine nanoclusters are adjacent to the skeleton metal N, are highly dispersed on the surface of the ZSM-5 matrix, and interact and tightly combine with the ZSM-5 matrix; the outer layer is an integral ZSM-5 hierarchical pore co-modified with ROx ultrafine nanoclusters and skeleton metal P inside and outside, the ROx ultrafine nanoclusters are adjacent to the skeleton metal P, are highly dispersed on the surface of the ZSM-5 matrix, and interact and tightly combine with the ZSM-5 matrix; the inner and outer layers have strong interaction and are tightly combined into an integral catalyst adsorbent; in addition, there is an organic film composed of organic amine or silane on the inner and outer surfaces of the adsorbent, which has a certain hydrophobicity.

[0059] The preparation method comprises the following steps:

[0060] S1: Preparation of framework lattice metal M-ZSM-5 nucleus solution A

[0061] S101: mixing a soluble salt of transition metal M and deionized water in a certain proportion, and then adding a certain amount of tetrapropylammonium hydroxide or tetrapropylammonium bromide (TPAOH / TPABr) after thermal radiation combined with ultrasound and magnetic stirring, and then again thermal radiation combined with ultrasound and magnetic stirring to obtain a mixture a;

[0062] S102: A certain amount of sodium hydroxide is dissolved in deionized water, and a certain amount of aluminum component is added, after thermal radiation combined with ultrasound and magnetic stirring, a certain amount of silicon component is added, and thermal radiation combined with ultrasound and magnetic stirring for a certain period of time to obtain a mixture b;

[0063] S103: slowly pouring mixture a into mixture b, while maintaining thermal radiation stirring and ultrasonic oscillation for a certain period of time, to obtain mixture c;

[0064] S104: The mixture c is transferred to a polytetrafluoroethylene reactor, and nucleated for a certain period of time under a certain pressure and thermal radiation combined with microwave-assisted heating to obtain an M-ZSM-5 crystal nucleus solution A.

[0065] S2: Preparation of N-ZSM-5 crystal nucleus solution B with surface metal M dispersed load

[0066] S201: adding a certain amount of heteronuclear metal N soluble salt to the crystal nucleus solution A, and obtaining a mixture d after thermal radiation combined with ultrasound and magnetic stirring;

[0067] S202: Transfer the mixture d to a polytetrafluoroethylene reactor, and nucleate for a certain period of time under a certain pressure and thermal radiation combined with microwave-assisted heating to obtain a crystal nucleus solution B of N-ZSM-5 with dispersed surface metal M load.

[0068] S3: Multi-level pores of ZSM-5 nanotubes co-modified with MOx ultrafine nanoclusters and skeleton metal N inner and outer surfaces

[0069] S301: Immerse a certain amount of carbon nanofibers, carbon nanotubes and other template agents in an organic amine or silane solvent of a certain concentration, filter and dry after immersing for a certain period of time.

[0070] S302: adding a certain amount of the dry product obtained in S301 to the crystal nucleus solution B, and obtaining a mixture f after thermal radiation combined with ultrasound and magnetic stirring;

[0071] S303: adding a certain amount of ethylenediaminetetraacetic acid (EDTA), cetyltrimethylammonium bromide (CTAB), polyquaternium salt and other solvents to the mixture f, and obtaining a mixture g after thermal radiation combined with ultrasound and magnetic stirring;

[0072] S304: After the mixture is dried by ultrasonic combined heating until it becomes a dry gel, it is transferred to a polytetrafluoroethylene reactor, crystallized for a certain period of time under a certain pressure and temperature, and calcined to obtain ZSM-5 multi-level porous nanotubes with inner and outer surfaces co-modified with skeleton lattice metal N and extra-skeleton ultrafine nanoclusters MOx, wherein M represents a transition metal element and N represents a transition metal or a rare earth metal element.

[0073] S4: Preparation of CO2 multi-level porous nanotube molecular sieve adsorbent

[0074] S401: According to the steps of S1 and S2, a crystal nucleus solution C is prepared, wherein the metal M in S1 is represented by the letter R, and the metal N in S2 is represented by the letter P.

[0075] S402: adding the ZSM-5 hierarchical porous nanotubes obtained in S304 to the crystal nucleus solution C, and adding a certain amount of ethylenediaminetetraacetic acid (EDTA), hexadecyltrimethylammonium bromide (CTAB), polyquaternary ammonium salt and other solvents, and obtaining a mixture h after thermal radiation combined with ultrasound and magnetic stirring;

[0076] S403: After the mixture is dried by ultrasonic combined heating until it becomes a dry glue, it is transferred to a polytetrafluoroethylene reactor, crystallized for a certain period of time under a certain pressure and temperature, and calcined to obtain MOx ultrafine nanoclusters / N-ZSM-5@ROx ultrafine nanoclusters / P-ZSM-5 nanotubes, wherein M and R represent transition metal elements, and N and P represent transition metals or rare earth metal elements.

[0077] S404: The ZSM-5 hierarchical pore nanotube adsorbent obtained in S403 is immersed in an organic amine or silane solvent of a certain concentration, and after being immersed for a certain period of time, filtered and dried to obtain a CO2 hierarchical pore nanotube molecular sieve adsorbent.

[0078] Preferably, the soluble salt of the transition metal M in step S101 may be a soluble salt such as nitrates, chlorides, organic salts, etc. of transition metals such as Mn, Ti, Fe, Ni, etc., or may be one or a combination of different soluble salts.

[0079] Preferably, the aluminum component in step S102 can be one or more of aluminum-containing substances such as aluminum chloride, sodium aluminate, aluminum hydroxide, and aluminum triethanolate.

[0080] Preferably, the molar ratio of each component in the mixture c of steps S103 and S104 is:

[0081] SiO2:TPAOH or TPABr = 100:(10-35);

[0082] SiO2:H2O=100: (1000-8000);

[0083] SiO2:Na2O=100:(10-30);

[0084] SiO2:M=100:(0.05-3);

[0085] SiO2:Al2O3=100:(10-600);

[0086] Preferably, the heteronuclear metal N soluble salt in step S201 may be soluble salts such as organic salts, nitrates, chlorides, etc. of transition metals such as Cu, Cr, Co, or rare earth metal elements such as La, Ce, or may be one or a combination of different soluble salts.

[0087] Preferably, the molar ratio of heteronuclear metal N to silicon component in the mixture d of step S202 is: SiO2:N=100:(0.05-3);

[0088] Preferably, in step S301, the solid-liquid ratio of the carbon nanofiber, carbon nanotube or other template agent to the organic amine or silane solution is 10:1, wherein the mass concentration of the organic amine or silane solution is 5-20%, and the drying temperature is 80-120°C;

[0089] Preferably, the organic amine or silane in step S301 is a solvent such as polyethyleneimine, phenylethylamine, trimethylchlorosilane, etc.;

[0090] Preferably, in step S302, the mass ratio of the amount of the template agent such as carbon nanofibers and carbon nanotubes added to the SiO2 in the mixture is (0.5-1.5):1;

[0091] Preferably, in steps S303 and S402, the mass ratio of the added amount of solvents such as ethylenediaminetetraacetic acid (EDTA), cetyltrimethylammonium bromide (CTAB), and polyquaternium salt to the mass ratio of SiO2 in the mixture is (0.05-0.8):1;

[0092] Preferably, the polyquaternary ammonium salt in step S303 can be polypropylene dimethyl ammonium chloride, polyacrylamide, N-vinyl pyrrolidone and quaternized vinyl imidazole copolymer, etc.

[0093] Preferably, during the crystallization process of steps S304 and S403, a small amount of deionized water is added to the reactor, the mass ratio of the added water to the dry glue is (0.5-2):1, the crystallization temperature is 140-200°C, and the crystallization time is 24-48h.

[0094] Preferably, the calcination process of steps S304 and S403 in air atmosphere is divided into three stages: in the first stage, the crystallized product is dried at 100-120°C for 2-3h; in the second stage, the temperature is slowly increased from 100-120°C to 300-400°C at a heating rate of 1-5°C, and kept constant for 3-5h; in the third stage, the calcination temperature is slowly increased to 500-700°C at a heating rate of 1-5°C, and kept constant for 4-6h.

[0095] Preferably, the metals R and P in step S401 may be the same as or different from the metals M and N in S1 and S2, respectively, or may be one or a combination of different soluble salts;

[0096] Preferably, in step S402, the mass ratio of the amount of ZSM-5 hierarchical porous nanotubes added to the amount of SiO2 in the mixture is (0.5-2):1;

[0097] Preferably, the solid-liquid ratio of the impregnation in step S404 is 10:1, wherein the mass concentration of the organic amine or silane solution is 5-20%, the drying temperature is 80-120° C., and the organic amine or silane is a solvent such as polyethyleneimine, phenylethylamine, or trimethylchlorosilane;

[0098] Preferably, in steps S1, S2, S3 and S4, the ultrasonic power is 50-300 W, the heating temperature is 50-80° C., the magnetic stirring speed is 400-800 r / min, and the ultrasonic combined with thermal radiation magnetic stirring time is 60-120 min;

[0099] Preferably, the nucleation in steps S1, S2 and S4 is carried out in a sealed reactor, the nucleation temperature is 80-120°C, the pressure is adjusted according to the temperature, the microwave power is 300-600W, and the nucleation time is 8-20h.

[0100] The invention is based on the heteronuclear in-situ anchoring substitution mechanism and adopts a two-step nucleation coordinated one-step dry colloid crystallization method to in-situ prepare a ZSM-5 molecular sieve co-modified with a framework metal and heteronuclear metal oxide ultrafine nanoclusters, wherein the framework metal ion radius is higher than the ion radius of the heteronuclear metal oxide; the framework metal is uniformly dispersed on the ZSM-5 framework, the heteronuclear metal oxide ultrafine nanoclusters are highly dispersed on the ZSM-5 surface, and more active sites such as oxygen vacancies and acidic sites are exposed on the surface of the ZSM-5 matrix.

[0101] The adsorbent developed by the present invention is ZSM-5, which is a multi-level pore nanotube molecular sieve. Template agents such as carbon nanotubes and carbon fibers are used, but are not limited to hard template agents, and also include carbon fibers synthesized by hydrothermal synthesis of high polymer soft template agents, and soft template agents such as polyquaternary ammonium salts are combined to prepare a multi-level pore nanotube structure molecular sieve. The adsorbent has a high specific surface area, developed pores, and good gas diffusion, which is conducive to the exposure of active sites and improves the adsorption capacity and adsorption efficiency.

[0102] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0103] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing a CO2 multi-level porous nanotube molecular sieve adsorbent, characterized in that: The following steps are involved: S1: using sodium hydroxide, tetrapropylammonium hydroxide or tetrapropylammonium bromide, a mixed solution of silicon component, aluminum component, ammonia water, polyquaternary ammonium salt, and transition metal salt as raw materials, preparing an M-ZSM-5 crystal nucleus solution A having a skeleton lattice metal; S2: adding heteronuclear metal N to the M-ZSM-5 crystal nucleus solution A, and nucleating under a certain pressure and temperature to prepare a crystal nucleus solution B of N-ZSM-5 with dispersed loading of surface metal M; S3: Add a certain amount of carbon nanofibers and carbon nanotube templates impregnated with organic amine and silane, ethylenediaminetetraacetic acid, hexadecyltrimethylammonium bromide, and polyquaternary ammonium salt solvent to the above-mentioned crystal nucleus solution B, stir and dry gel, transfer to a polytetrafluoroethylene reactor, crystallize under a certain pressure and temperature, and obtain ZSM-5 nanotubes co-modified with skeleton lattice metal N and extra-skeleton ultrafine nanoclusters MOx on the inner and outer surfaces after three-stage calcination; immerse the obtained ZSM-5 nanotubes in an organic amine or silane solvent, and obtain a CO2 multi-level porous nanotube molecular sieve adsorbent after drying; Among them, M represents a transition metal element, N represents a transition metal or a rare earth metal element, N-ZSM-5 is a multi-level porous nanotube molecular sieve with an MFI structure, the MOx ultrafine nanocluster is an ultrafine nanocluster oxide of metal M in a highly dispersed state, and N is a metal element whose metal ion radius is higher than that of M.

2. The preparation method according to claim 1, characterized in that: The method of step S1 specifically includes the following sub-steps: S101: mixing a soluble salt of a transition metal M and deionized water in a certain proportion, and subjecting the mixture to thermal radiation combined with ultrasound and magnetic stirring, and then adding a certain amount of tetrapropylammonium hydroxide or tetrapropylammonium bromide, and subjecting the mixture to thermal radiation combined with ultrasound and magnetic stirring again to obtain a mixture a; S102: dissolving a certain amount of sodium hydroxide in deionized water, adding a certain amount of aluminum component, adding a certain amount of silicon component after thermal radiation combined with ultrasound and magnetic stirring, and thermal radiation combined with ultrasound and magnetic stirring for a certain period of time to obtain a mixture b; S103: slowly pouring mixture a into mixture b while maintaining thermal radiation stirring and ultrasonic vibration for a certain period of time to obtain mixture c; S104: transferring the mixture c to a polytetrafluoroethylene reactor, and nucleating it for a certain period of time under a certain pressure and thermal radiation combined with microwave-assisted heating to obtain an M-ZSM-5 crystal nucleus solution A; The molar ratio of each component in the mixture c of steps S103 and S104 is: SiO2:TPAOH or TPABr = 100: (10-35); SiO2:H2 O=100: (1000-8000); SiO2:Na2 O=100: (10-30); SiO2: M = 100: (0.05-3); SiO2 :Al2 O3 =100:(10-600).

3. The preparation method according to claim 1, characterized in that: The method of step S2 specifically includes the following sub-steps: S201: adding a certain amount of heteronuclear metal N soluble salt to the crystal nucleus solution A, and obtaining a mixture d after thermal radiation combined with ultrasound and magnetic stirring; S202: Transfer the mixture d to a polytetrafluoroethylene reactor, and nucleate for a certain period of time under a certain pressure and thermal radiation combined with microwave-assisted heating to obtain a crystal nucleus solution B of N-ZSM-5 with dispersed loading of surface metal M; In step S202, the molar ratio of the heteronuclear metal N to the silicon component in the mixture d is: SiO2:N=100:(0.05-3).

4. The preparation method according to claim 1, characterized in that: The method of step S3 specifically includes the following sub-steps: S301: immersing a certain amount of carbon nanofibers or carbon nanotube templates in an organic amine or silane solvent of a certain concentration, filtering and drying after immersion for a certain period of time; S302: adding the dried product obtained in S301 to the crystal nucleus solution B, and obtaining a mixture f after thermal radiation combined with ultrasound and magnetic stirring; S303: adding a certain amount of ethylenediaminetetraacetic acid, hexadecyltrimethylammonium bromide and polyquaternary ammonium salt solvent to the mixture f, and obtaining a mixture g after thermal radiation combined with ultrasound and magnetic stirring; S304: After the mixture is dried by ultrasonic combined heating until it becomes a dry gel, it is transferred to a polytetrafluoroethylene reactor, crystallized for a certain period of time under a certain pressure and temperature, and calcined to obtain a ZSM-5 hierarchical porous nanotube with the inner and outer surfaces of the skeleton lattice metal N and the extra-skeleton ultrafine nanoclusters MOx co-modified; S305: The ZSM-5 hierarchical pore nanotube adsorbent obtained in S304 is immersed in an organic amine or silane solvent of a certain concentration, and after being immersed for a certain period of time, filtered and dried to obtain a CO2 hierarchical pore nanotube molecular sieve adsorbent.

5. The preparation method according to claim 4, characterized in that: In step S301, the solid-liquid ratio of the carbon nanofibers and carbon nanotubes template to the organic amine or silane solution is 10:1, wherein the mass concentration of the organic amine or silane solution is 5-20%, and the drying temperature is 80-120°C; Step S302: the mass ratio of the amount of carbon nanofibers and carbon nanotube templates added to the SiO2 in the mixture is (0.5-1.5):1; Step S303: the mass ratio of the added amount of ethylenediaminetetraacetic acid, hexadecyltrimethylammonium bromide, and polyquaternium salt solvent to the mass ratio of SiO2 in the mixture is (0.05-0.8):1; In step S304, during the crystallization process, a small amount of deionized water is added to the reaction kettle, the mass ratio of the added water to the dry glue is (0.5-2):1, the crystallization temperature is 140-200°C, and the crystallization time is 24-48h; The calcination process in step S304 under air atmosphere is divided into three stages: in the first stage, the crystallized product is dried at 100-120°C for 2-3 hours; in the second stage, the temperature is slowly increased from 100-120°C to 300-400°C at a heating rate of 1-5°C, and the temperature is kept constant for 3-5 hours; in the third stage, the calcination temperature is slowly increased to 500-700°C at a heating rate of 1-5°C, and the temperature is kept constant for 4-6 hours; In step S305, the immersion solid-liquid ratio is 10:1, wherein the mass concentration of the organic amine or silane solution is 5-20%, and the drying temperature is 80-120°C.

6. The preparation method according to claim 1, characterized in that: In steps S1, S2 and S3, the ultrasonic power is 50-300 W, the heating temperature is 50-80° C., the magnetic stirring speed is 400-800 r / min, and the ultrasonic combined with thermal radiation magnetic stirring time is 60-120 min; In steps S1 and S2, the nucleation is carried out in a sealed reactor, the nucleation temperature is 80-120° C., the pressure is adjusted according to the temperature, the microwave power is 300-600 W, and the nucleation time is 8-20 h.

7. The preparation method according to claim 4, characterized in that: The method further comprises step S4, wherein the method of step S4 specifically comprises the following sub-steps: S401: According to the steps of S1 and S2, a crystal nucleus solution C is prepared, wherein the metal M in S1 is represented by the letter R, and the metal N in S2 is represented by the letter P; S402: adding the ZSM-5 hierarchical porous nanotubes obtained in S304 to the crystal nucleus solution C, and adding a certain amount of ethylenediaminetetraacetic acid, hexadecyltrimethylammonium bromide, and polyquaternary ammonium salt solvent, and obtaining a mixture h after thermal radiation combined with ultrasound and magnetic stirring; S403: After the mixture is dried by ultrasonic combined heating until it becomes a dry gel, it is transferred to a polytetrafluoroethylene reactor, crystallized for a certain period of time under a certain pressure and temperature, and calcined to obtain MOx ultrafine nanoclusters / N-ZSM-5@ROx ultrafine nanoclusters / P-ZSM-5 nanotubes; S404: impregnating the ZSM-5 hierarchical nanotube adsorbent obtained in S403 into an organic amine or silane solvent of a certain concentration, filtering and drying after impregnation for a certain period of time to obtain a CO2 hierarchical nanotube molecular sieve adsorbent; In step S402, the mass ratio of the amount of ZSM-5 hierarchical porous nanotubes added to the SiO2 in the mixture is (0.5-2):1; In step S404, the immersion solid-liquid ratio is 10:1, wherein the mass concentration of the organic amine or silane solution is 5-20%, and the drying temperature is 80-120°C.

8. A CO2 hierarchical nanotube molecular sieve adsorbent, characterized in that: The adsorbent is a single-shell adsorbent, and its general formula is U @ MOx ultrafine nanoclusters / N-ZSM-5 @ Y nanotubes, wherein M represents a transition metal element, N represents a transition metal or a rare earth metal element, and U and Y represent organic amines or silanes. The adsorbent is an integral nanotube molecular sieve adsorbent co-modified with MOx ultrafine nanoclusters and skeleton metal N inside and outside, wherein the MOx ultrafine nanoclusters are adjacent to the skeleton metal N and are highly dispersed on the surface of the ZSM-5 matrix, and interact and tightly bind with the ZSM-5 matrix. In addition, there is an organic film composed of organic amines or silanes on the inner and outer surfaces of the adsorbent, respectively.

9. A CO2 hierarchical nanotube molecular sieve adsorbent, characterized in that: The adsorbent is a double-shell adsorbent, and its general formula is U @ MOx ultrafine nanocluster / N-ZSM-5@ROx ultrafine nanocluster / P-ZSM-5 @ Y nanotube, wherein M and R represent transition metal elements, N and P represent transition metals or rare earth metal elements, U and Y represent organic amines or silanes, N-ZSM-5 and P-ZSM-5 are multi-level porous molecular sieves with MFI structure, MOx and ROx ultrafine nanocluster are ultrafine nanocluster oxides of transition metals, which are in a highly dispersed state, and N and P are metal elements whose metal ion radii are respectively larger than M and R; the inner layer of the adsorbent is an integral ZSM-5 multi-level porous nanotube co-modified with MOx ultrafine nanocluster and skeleton metal N inside and outside, and MOx ultrafine nanocluster is a kind of monolithic ZSM-5 multi-level porous nanotube. The fine nanoclusters are close to the skeleton metal N and are highly dispersed on the surface of the ZSM-5 matrix, and interact and bind tightly with the ZSM-5 matrix; the outer layer is an integral ZSM-5 multi-level pore co-modified with ROx ultrafine nanoclusters and skeleton metal P inside and outside, the ROx ultrafine nanoclusters are close to the skeleton metal P and are highly dispersed on the surface of the ZSM-5 matrix, and interact and bind tightly with the ZSM-5 matrix; the inner and outer layers have a strong interaction and are tightly combined into an integral catalyst and adsorbent; there is an organic film composed of organic amine or silane on the inner and outer surfaces of the adsorbent respectively.