Flame retardant polystyrene board and preparation method thereof

By using chlorinated polyethylene, phenolic resin, expanded graphite, polyphenylene sulfide fiber and modified flame retardant and other auxiliary materials in the polystyrene board, a stable fireproof layer is formed, which solves the problem of unstable fireproof performance of the polystyrene board. Its hardness, tensile strength and thermal insulation properties are improved, ensuring safety and stability of flame retardant properties.

CN117986760BActive Publication Date: 2024-10-29QINGDAO WANXING BUILDING MATERIALS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410155575.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-04
Publication Date
2024-10-29
Estimated Expiration
2044-02-04

AI Technical Summary

Technical Problem

The fireproof performance of existing polystyrene boards is unstable and tends to decrease with extended use time. Moreover, it has poor heat resistance and is easy to burn, posing potential safety hazards.

Method used

Using chlorinated polyethylene, phenolic resin, expanded graphite, polyphenylene sulfide fiber and modified flame retardant and other auxiliary materials, through the dispersion and wrapping technology of modified flame retardant, the flame retardant performance and mechanical properties of polystyrene board are improved. Form a more stable fire protection layer.

Benefits of technology

The hardness, tensile strength, thermal insulation performance and flame retardant performance of the polystyrene board are significantly improved, ensuring the comprehensive performance improvement and safety of the material, the flame retardant performance is stable, and the spread of fire is avoided.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a flame retardant polystyrene board and a preparation method thereof, and belongs to the technical field of composite materials. The flame retardant polystyrene board is made of the following raw materials: polystyrene, chlorinated polyethylene, phenolic resin, expanded graphite, polyphenylene sulfide fiber, modified flame retardant, foaming agent, compatibilizer, antioxidant, and lubricant. Among them, the modified flame retardant is made of melamine cyanurate as the main material, and is prepared by polymethacryloyloxyethyl trimethyl ammonium chloride treatment, water-based polyaspartic acid ester resin treatment and lysine diisocyanate curing in sequence. Compared with the unmodified flame retardant, the modified flame retardant has better compatibility with the polystyrene board matrix, can ensure the comprehensive properties of the polystyrene board such as mechanics, and further improve the flame retardant properties of the polystyrene board.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and particularly relates to a flame retardant polystyrene board and a preparation method thereof. Background Art

[0002] Polystyrene board, also known as EPS board, is based on expandable polystyrene raw materials and is made through a series of processes such as pre-expansion, aging, molding, drying and cutting. It is widely used in many fields, including construction, packaging, refrigeration, freezing, shipping, industrial casting, etc., mainly used as insulation, heat insulation, sound insulation and earthquake resistance materials. Polystyrene board has a series of advantages, such as light weight, low price, sound insulation, earthquake resistance, low thermal conductivity, good insulation, low water absorption, easy molding, etc. These characteristics make it popular in the construction industry, providing a light, economical and efficient insulation solution. Although polystyrene board performs well in many aspects, as an organic material, it has poor heat resistance and is easy to burn. During the combustion process, polystyrene board will generate a lot of heat and dripping, which may accelerate the spread of fire, which requires special attention in terms of fire safety. Therefore, while ensuring the advantages of thermal insulation, heat insulation and earthquake resistance of the material itself, it is very necessary to improve the polystyrene board material and enhance its flame retardant and fireproof properties.

[0003] Chinese patent CN104016711B discloses a method for making an inorganic modified polystyrene board, comprising the following steps: preparing fireproof raw materials, including water glass or silica sol, light calcium carbonate, heavy calcium carbonate or kaolin, polyacrylamide, sodium dodecyl sulfate or sodium dodecyl sulfonate, carbon dioxide, and silicon aerogel, stirring the raw materials evenly according to the proportion, then pouring the fireproof raw materials from the top on the polystyrene board to evenly penetrate and gradually solidify, and then taking it out and dehydrating it by drying or airing to form an inorganic modified polystyrene board; this patent utilizes the gaps between polystyrene particles to penetrate the fireproof raw materials into the fine closed pores, and coats the surface of the polystyrene particles to form a fireproof layer to improve the fireproof performance. Chinese patent CN104151730B discloses a modified polystyrene board and its preparation method, including: mixing pre-expanded polystyrene particles with coating material and curing agent and then flattening, using steam to blow the flattened mixture, and then pressing it into a board, wherein the coating material includes phenolic resin, chemical foaming agent, emulsifier and inorganic flame retardant, and the inorganic flame retardant is one or more of magnesium hydroxide, aluminum hydroxide, silicon dioxide, decabromodiphenyl ether, and MCA; this patent improves its oxygen index, compression strength and tensile strength by bonding the coating material to the surface of polystyrene, so that the polystyrene board has a certain flame retardant ability. However, the above methods are all made by coating or coating the surface of polystyrene with raw materials containing flame retardants, which makes the fire resistance of the modified polystyrene board unstable, and the performance will decrease with the extension of the use time. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a flame retardant polystyrene board, which ensures the comprehensive mechanical properties of the polystyrene board by adding a modified flame retardant having better compatibility with the polystyrene board matrix, and further improves the flame retardant properties of the polystyrene board. The present invention also provides a method for preparing the flame retardant polystyrene board, which has a simple process, and the prepared flame retardant polystyrene board has stable performance and high safety.

[0005] A flame retardant polystyrene board is made of the following raw materials: polystyrene, chlorinated polyethylene, phenolic resin, expanded graphite, polyphenylene sulfide fiber, modified flame retardant, foaming agent, compatibilizer, antioxidant and lubricant.

[0006] The present invention adopts chlorinated polyethylene, phenolic resin, expanded graphite and polyphenylene sulfide fiber as auxiliary materials of polystyrene to prepare flame-retardant polystyrene board, the addition of chlorinated polyethylene helps to improve the strength and impact resistance of polystyrene board, and endows it with more superior mechanical properties; the introduction of phenolic resin helps to enhance the hardness and tensile strength of polystyrene board, making it more durable in application; the use of expanded graphite improves the thermal insulation performance of polystyrene board, and creates a better thermal insulation effect for it; the addition of polyphenylene sulfide fiber further improves the strength, thermal stability and flame retardant performance of polystyrene board. The synergistic effect of these auxiliary materials provides comprehensive performance improvement for polystyrene board, so that polystyrene board is comprehensively improved in terms of hardness, tensile strength, thermal insulation and flame retardant performance.

[0007] Preferably, a flame retardant polystyrene board is made of the following raw materials: 70-100 parts by weight of polystyrene, 5-15 parts by weight of chlorinated polyethylene, 2-8 parts by weight of phenolic resin, 8-12 parts by weight of expanded graphite, 8-12 parts by weight of polyphenylene sulfide fiber, 10-15 parts by weight of modified flame retardant, 5-10 parts by weight of foaming agent, 1-3 parts by weight of compatibilizer, 0.5-1.5 parts by weight of antioxidant, and 1-2 parts by weight of lubricant.

[0008] Preferably, the modified flame retardant is prepared by the following method:

[0009] Polyethylene glycol and sodium polystyrene sulfonate are added to water and mixed evenly, and then melamine cyanurate is added and stirred to obtain dispersion X; magnesium chloride and polymethacryloyloxyethyl trimethyl ammonium chloride are added to the dispersion X and stirred continuously, and then an aqueous polyaspartic acid ester resin aqueous dispersion is added and heated and stirred to obtain a treatment liquid Y; L-lysine diisocyanate aqueous dispersion is added to the treatment liquid Y for curing, and after curing, the mixture is filtered, washed with water, and dried to obtain a modified flame retardant.

[0010] Hydrophobic powder flame retardants such as melamine cyanurate, melamine borate, triphenyl phosphate, tetrabromobisphenol A, etc. have large surface energy, and their surfaces easily adsorb more air, which increases the distance between powder particles, resulting in a small packing density, which is not conducive to direct application. The present invention first uses a combination of polyethylene glycol and sodium polystyrene sulfonate as a dispersant to uniformly disperse the hydrophobic powder flame retardant melamine cyanurate in the aqueous phase, which is conducive to the smooth progress of subsequent modification; then it is modified by polymethacryloyloxyethyl trimethylammonium chloride and aqueous polyaspartic acid ester resin in turn, thereby forming a polyelectrolyte layer and an aqueous polyurea layer on the surface of the hydrophobic powder flame retardant. The aqueous polyaspartic acid ester containing hydrophilic groups such as polyether groups and amino groups is more hydrophilic than the hydrophobic powder flame retardant, and can reduce The surface energy is lowered to reduce the air adsorbed on the surface of the powder, and the bulk density of the powder is increased. At the same time, the aqueous polyurea layer and the polyelectrolyte cooperate with each other through hydrogen bonds and intermolecular forces, effectively realizing the uniform coating of the surface of the hydrophobic powder flame retardant by the polymer. Finally, the polyurea layer is cured by L-lysine diisocyanate to form a more stable interface force, making the coating layer more compact, and the thermal stability and bulk density of the hydrophobic powder flame retardant are further improved, which is helpful to improve the processability and flame retardant efficiency of the hydrophobic powder flame retardant. In addition, the addition of inorganic salt magnesium chloride can adjust the ionic strength of the water phase, which is beneficial to improve the coating rate of polymethacryloyloxyethyl trimethyl ammonium chloride and aqueous polyaspartic acid ester resin, and the coating layer is thin, which will not significantly increase the particle size of the powder flame retardant, and the flame retardant effect of the flame retardant can be guaranteed when added to the polystyrene board matrix, and at the same time, it has better compatibility with the polystyrene board matrix, and can improve the mechanical and other comprehensive properties of the polystyrene board.

[0011] Preferably, the modified flame retardant is prepared by the following method:

[0012] 0.2-0.5 parts by weight of polyethylene glycol and 0.1-0.2 parts by weight of sodium polystyrene sulfonate are added to 300-600 parts by weight of water and mixed evenly, and then 100-150 parts by weight of melamine cyanurate are added and stirred at 30-35° C. and 700-1000 r / min for 120-160 min to obtain a dispersion X; 1-3 parts by weight of magnesium chloride and 0.3-0.6 parts by weight of polymethacryloyloxyethyl trimethyl ammonium chloride are added to the dispersion X and stirred for 30-60 min. in, then add 10-30 parts by weight of aqueous polyaspartic acid ester resin aqueous dispersion, heat to 40-50°C and stir for 80-120min to obtain treatment liquid Y; add 20-30 parts by weight of L-lysine diisocyanate aqueous dispersion to the above treatment liquid Y and keep warm at 62-68°C for 50-100min, then heat to 80-88°C and keep warm for 150-200min to cure, after completion, filter, wash with water, and dry at 90-100°C for 10-15h to obtain a modified flame retardant.

[0013] Preferably, the polyethylene glycol is polyethylene glycol 4000.

[0014] Preferably, the concentration of the aqueous polyaspartic acid ester resin aqueous dispersion is 1-5 wt %.

[0015] Preferably, the concentration of the L-lysine diisocyanate aqueous dispersion is 0.1-0.3 wt %.

[0016] Preferably, the compatibilizer is SEBS-g-MAH.

[0017] Preferably, the foaming agent is any one of butane foaming agent, pentane foaming agent and pentafluoropropane foaming agent.

[0018] Preferably, the lubricant is any one of calcium stearate, polyethylene wax and silicone powder.

[0019] Preferably, the antioxidant is any one of antioxidant 1010, antioxidant 2246, and antioxidant 1076.

[0020] The present invention also provides a method for preparing a flame retardant polystyrene board, comprising the following steps:

[0021] According to the formula, polystyrene, chlorinated polyethylene, phenolic resin and compatibilizer are weighed and mixed in an open mill at 190-210°C for 10-30 minutes to obtain a blend; then the blend is evenly mixed with expanded graphite, polyphenylene sulfide fiber, modified flame retardant, antioxidant and lubricant, and then melt-mixed in a twin-screw extruder, extruded and pelletized to obtain polystyrene board particles; the polystyrene board particles are mixed with a foaming agent and placed in an extruder for extrusion molding, and dried at 40-60°C for 2-5 hours to obtain the flame-retardant polystyrene board.

[0022] Preferably, the process conditions of the twin-screw extruder are: the temperature range of each zone is 200-240° C., and the main engine speed is 100-300 r / min.

[0023] In some embodiments, polystyrene is purchased from Shanghai Yiding Plastic Co., Ltd., general-purpose grade, brand PG-383. Phenolic resin is purchased from Shandong Shengquan New Materials Co., Ltd., general-purpose grade, brand PF2828. Chlorinated polyethylene is purchased from Shandong Bangtai Petrochemical (Group) Co., Ltd., brand CPE135A. SEBS-g-MAH, melt index is 0.2-0.8 g / 10 min, grafting rate is 1.5-2%.

[0024] Beneficial effects of the present invention:

[0025] (1) The present invention uses chlorinated polyethylene, phenolic resin, expanded graphite and polyphenylene sulfide fiber as auxiliary materials of polystyrene to prepare flame-retardant polystyrene board. The synergistic effect of these auxiliary materials provides comprehensive performance improvement for the polystyrene board, so that the polystyrene board has been comprehensively improved in terms of hardness, tensile strength, thermal insulation and flame retardancy.

[0026] (2) The flame retardant polystyrene board prepared by the present invention has excellent flame retardant properties and mechanical properties. The modified flame retardant used is a hydrophobic powder flame retardant melamine cyanurate modified by polymethacryloyloxyethyl trimethylammonium chloride and aqueous polyaspartic acid ester resin in sequence, thereby forming a polyelectrolyte layer and an aqueous polyurea layer on its surface. Adding it to the polystyrene board matrix can ensure the flame retardant effect of the flame retardant, and at the same time has better compatibility with the polystyrene board matrix, which can improve the comprehensive properties of the polystyrene board such as mechanics. DETAILED DESCRIPTION

[0027] The above-mentioned invention contents of the present invention are further described in detail below in conjunction with specific implementation methods. The embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the contents of the present invention and implement them accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit and essence of the present invention should be included in the protection scope of the present invention.

[0028] Example 1

[0029] A flame retardant polystyrene board is made from the following raw materials:

[0030] 85 parts by weight of polystyrene, 10 parts by weight of chlorinated polyethylene, 5 parts by weight of phenolic resin, 10 parts by weight of expanded graphite (200 mesh), 10 parts by weight of polyphenylene sulfide fiber (length 0.5 mm, diameter 1.5 μm), 10.5 parts by weight of modified flame retardant, 8 parts by weight of butane foaming agent, 2.5 parts by weight of compatibilizer SEBS-g-MAH, 1 part by weight of antioxidant 1010, and 1.5 parts by weight of lubricant calcium stearate.

[0031] The modified flame retardant is prepared by the following method:

[0032] 0.38 parts by weight of polyethylene glycol 4000 and 0.12 parts by weight of sodium polystyrene sulfonate (molecular weight 70,000) were added to 500 parts by weight of water and mixed evenly, and then 120 parts by weight of melamine cyanurate were added and stirred at 32° C. and 800 r / min for 150 minutes to obtain dispersion X; 2.4 parts by weight of magnesium chloride and 0.55 parts by weight of polymethacryloyloxyethyl trimethylammonium chloride (molecular weight 200,000) were added to the above dispersion X and stirred for 50 minutes, and then 20 parts by weight of 3wt% aqueous polyaspartic acid ester resin aqueous dispersion were added, and the temperature was raised to 45° C. and stirred for 100 minutes to obtain treatment liquid Y; 25 parts by weight of 0.2wt% L-lysine diisocyanate aqueous dispersion were added to the above treatment liquid Y and kept warm at 66° C. for 80 minutes, and then heated to 82° C. and kept warm for 160 minutes for curing, and after the curing, filtered, washed with water, and dried at 95° C. for 12 hours to obtain a modified flame retardant. Wherein, the water-based polyaspartic acid ester resin is prepared according to the method of Example 1 in patent CN111303368B.

[0033] A method for preparing a flame retardant polystyrene board comprises the following steps:

[0034] According to the formula, polystyrene, chlorinated polyethylene, phenolic resin and compatibilizer are weighed and mixed in an open mill at 200° C. for 15 minutes to obtain a blend; then the blend is evenly mixed with expanded graphite, polyphenylene sulfide fiber, modified flame retardant, antioxidant and lubricant, and then melt-mixed in a twin-screw extruder, extruded and pelletized to obtain polystyrene board particles; the polystyrene board particles are mixed with a foaming agent and placed in an extruder for extrusion molding, and dried at 50° C. for 4 hours to obtain the flame-retardant polystyrene board.

[0035] Among them, the process conditions of the twin-screw extruder are: the temperature of zone I is 220°C, the temperature of zone II is 225°C, the temperature of zone III is 230°C, the temperature of zone IV is 230°C, the temperature of zone V is 235°C, and the main engine speed is 200r / min.

[0036] Example 2

[0037] A flame retardant polystyrene board is made from the following raw materials:

[0038] 85 parts by weight of polystyrene, 10 parts by weight of chlorinated polyethylene, 5 parts by weight of phenolic resin, 10 parts by weight of expanded graphite (200 mesh), 10 parts by weight of polyphenylene sulfide fiber (length 0.5 mm, diameter 1.5 μm), 10.5 parts by weight of modified flame retardant, 8 parts by weight of butane foaming agent, 2.5 parts by weight of compatibilizer SEBS-g-MAH, 1 part by weight of antioxidant 1010, and 1.5 parts by weight of lubricant calcium stearate.

[0039] The modified flame retardant is prepared by the following method:

[0040] 0.38 parts by weight of polyethylene glycol 4000 and 0.12 parts by weight of sodium polystyrene sulfonate (molecular weight 70000) were added to 500 parts by weight of water and mixed evenly, and then 120 parts by weight of melamine cyanurate were added and stirred at 32° C. and 800 r / min for 150 minutes to obtain a dispersion X; 2.4 parts by weight of magnesium chloride and 0.55 parts by weight of polymethacryloyloxyethyltrimethylammonium chloride (molecular weight 200000) were added to the above dispersion X and stirred for 50 minutes, and the temperature was raised to 45° C. and stirred for 100 minutes. After the mixture was filtered, washed with water, and dried at 95° C. for 12 hours to obtain a modified flame retardant.

[0041] A method for preparing a flame retardant polystyrene board comprises the following steps:

[0042] According to the formula, polystyrene, chlorinated polyethylene, phenolic resin and compatibilizer are weighed and mixed in an open mill at 200° C. for 15 minutes to obtain a blend; then the blend is evenly mixed with expanded graphite, polyphenylene sulfide fiber, modified flame retardant, antioxidant and lubricant, and then melt-mixed in a twin-screw extruder, extruded and pelletized to obtain polystyrene board particles; the polystyrene board particles are mixed with a foaming agent and placed in an extruder for extrusion molding, and dried at 50° C. for 4 hours to obtain the flame-retardant polystyrene board.

[0043] Among them, the process conditions of the twin-screw extruder are: the temperature of zone I is 220°C, the temperature of zone II is 225°C, the temperature of zone III is 230°C, the temperature of zone IV is 230°C, the temperature of zone V is 235°C, and the main engine speed is 200r / min.

[0044] Example 3

[0045] A flame retardant polystyrene board is made from the following raw materials:

[0046] 85 parts by weight of polystyrene, 10 parts by weight of chlorinated polyethylene, 5 parts by weight of phenolic resin, 10 parts by weight of expanded graphite (200 mesh), 10 parts by weight of polyphenylene sulfide fiber (length 0.5 mm, diameter 1.5 μm), 10.5 parts by weight of modified flame retardant, 8 parts by weight of butane foaming agent, 2.5 parts by weight of compatibilizer SEBS-g-MAH, 1 part by weight of antioxidant 1010, and 1.5 parts by weight of lubricant calcium stearate.

[0047] The modified flame retardant is prepared by the following method:

[0048] 0.38 parts by weight of polyethylene glycol 4000 and 0.12 parts by weight of sodium polystyrene sulfonate (molecular weight 70000) were added to 500 parts by weight of water and mixed evenly, and then 120 parts by weight of melamine cyanurate were added and stirred at 32°C and 800 r / min for 150 minutes to obtain dispersion X; 2.4 parts by weight of magnesium chloride were added to the above dispersion X and stirred for 50 minutes, and then 20 parts by weight of 3wt% aqueous polyaspartic acid ester resin aqueous dispersion were added, and the temperature was raised to 45°C and stirred for 100 minutes to obtain treatment liquid Y; 25 parts by weight of 0.2wt% L-lysine diisocyanate aqueous dispersion were added to the above treatment liquid Y and kept warm at 66°C for 80 minutes, and then heated to 82°C and kept warm for 160 minutes for curing, and after the curing, filtered, washed with water, and dried at 95°C for 12 hours to obtain a modified flame retardant. Wherein, the water-based polyaspartic acid ester resin is prepared according to the method of Example 1 in patent CN111303368B.

[0049] A method for preparing a flame retardant polystyrene board comprises the following steps:

[0050] According to the formula, polystyrene, chlorinated polyethylene, phenolic resin and compatibilizer are weighed and mixed in an open mill at 200° C. for 15 minutes to obtain a blend; then the blend is evenly mixed with expanded graphite, polyphenylene sulfide fiber, modified flame retardant, antioxidant and lubricant, and then melt-mixed in a twin-screw extruder, extruded and pelletized to obtain polystyrene board particles; the polystyrene board particles are mixed with a foaming agent and placed in an extruder for extrusion molding, and dried at 50° C. for 4 hours to obtain the flame-retardant polystyrene board.

[0051] Among them, the process conditions of the twin-screw extruder are: the temperature of zone I is 220°C, the temperature of zone II is 225°C, the temperature of zone III is 230°C, the temperature of zone IV is 230°C, the temperature of zone V is 235°C, and the main engine speed is 200r / min.

[0052] Example 4

[0053] A flame retardant polystyrene board is made from the following raw materials:

[0054] 85 parts by weight of polystyrene, 10 parts by weight of chlorinated polyethylene, 5 parts by weight of phenolic resin, 10 parts by weight of expanded graphite (200 mesh), 10 parts by weight of polyphenylene sulfide fiber (length 0.5 mm, diameter 1.5 μm), 10.5 parts by weight of modified flame retardant, 8 parts by weight of butane foaming agent, 2.5 parts by weight of compatibilizer SEBS-g-MAH, 1 part by weight of antioxidant 1010, and 1.5 parts by weight of lubricant calcium stearate.

[0055] The modified flame retardant is prepared by the following method:

[0056] 0.38 parts by weight of polyethylene glycol 4000 and 0.12 parts by weight of sodium polystyrene sulfonate (molecular weight 70000) were added to 500 parts by weight of water and mixed evenly, and then 120 parts by weight of cyanuric acid melamine were added and stirred at 32°C and 800r / min for 150 minutes to obtain dispersion X; 2.4 parts by weight of magnesium chloride and 0.55 parts by weight of polymethacryloyloxyethyl trimethylammonium chloride (molecular weight 200000) were added to the above dispersion X and stirred for 50 minutes, and then 20 parts by weight of 3wt% aqueous polyaspartic acid ester resin aqueous dispersion were added, the temperature was raised to 45°C and stirred for 100 minutes, and then filtered, washed with water, and dried at 95°C for 12 hours to obtain a modified flame retardant. Wherein, the aqueous polyaspartic acid ester resin was prepared according to the method of Example 1 in patent CN111303368B.

[0057] A method for preparing a flame retardant polystyrene board comprises the following steps:

[0058] According to the formula, polystyrene, chlorinated polyethylene, phenolic resin and compatibilizer are weighed and mixed in an open mill at 200° C. for 15 minutes to obtain a blend; then the blend is evenly mixed with expanded graphite, polyphenylene sulfide fiber, modified flame retardant, antioxidant and lubricant, and then melt-mixed in a twin-screw extruder, extruded and pelletized to obtain polystyrene board particles; the polystyrene board particles are mixed with a foaming agent and placed in an extruder for extrusion molding, and dried at 50° C. for 4 hours to obtain the flame-retardant polystyrene board.

[0059] Among them, the process conditions of the twin-screw extruder are: the temperature of zone I is 220°C, the temperature of zone II is 225°C, the temperature of zone III is 230°C, the temperature of zone IV is 230°C, the temperature of zone V is 235°C, and the main engine speed is 200r / min.

[0060] Example 5

[0061] A flame retardant polystyrene board is made from the following raw materials:

[0062] 85 parts by weight of polystyrene, 10 parts by weight of chlorinated polyethylene, 5 parts by weight of phenolic resin, 10 parts by weight of expanded graphite (200 mesh), 10 parts by weight of polyphenylene sulfide fiber (length 0.5 mm, diameter 1.5 μm), 10.5 parts by weight of modified flame retardant, 8 parts by weight of butane foaming agent, 2.5 parts by weight of compatibilizer SEBS-g-MAH, 1 part by weight of antioxidant 1010, and 1.5 parts by weight of lubricant calcium stearate.

[0063] The modified flame retardant is prepared by the following method:

[0064] Add 120 parts by weight of cyanuric acid melamine to 500 parts by weight of water and stir at 32°C and 800r / min for 150min to obtain dispersion X; add 2.4 parts by weight of magnesium chloride and 0.55 parts by weight of polymethacryloyloxyethyl trimethyl ammonium chloride (molecular weight 200000) to the above dispersion X and continue stirring for 50min, then add 20 parts by weight of 3wt% aqueous polyaspartic acid ester resin aqueous dispersion, heat to 45°C and stir for 100min to obtain treatment liquid Y; add 25 parts by weight of 0.2wt% L-lysine diisocyanate aqueous dispersion to the above treatment liquid Y and keep warm at 66°C for 80min, then heat to 82°C and keep warm for 160min to cure, filter, wash with water, and dry at 95°C for 12h to obtain modified flame retardant. Wherein, the aqueous polyaspartic acid ester resin is prepared according to the method of Example 1 in patent CN111303368B.

[0065] A method for preparing a flame retardant polystyrene board comprises the following steps:

[0066] According to the formula, polystyrene, chlorinated polyethylene, phenolic resin and compatibilizer are weighed and mixed in an open mill at 200° C. for 15 minutes to obtain a blend; then the blend is evenly mixed with expanded graphite, polyphenylene sulfide fiber, modified flame retardant, antioxidant and lubricant, and then melt-mixed in a twin-screw extruder, extruded and pelletized to obtain polystyrene board particles; the polystyrene board particles are mixed with a foaming agent and placed in an extruder for extrusion molding, and dried at 50° C. for 4 hours to obtain the flame-retardant polystyrene board.

[0067] Among them, the process conditions of the twin-screw extruder are: the temperature of zone I is 220°C, the temperature of zone II is 225°C, the temperature of zone III is 230°C, the temperature of zone IV is 230°C, the temperature of zone V is 235°C, and the main engine speed is 200r / min.

[0068] Test Example 1

[0069] The impact strength of the flame retardant polystyrene board was measured according to the standard GB / T 1843-2008 "Determination of Izod Impact Strength of Plastics". Ten groups were tested in parallel, and the average value was calculated. The results are shown in Table 1.

[0070] Table 1. Impact strength test results of polystyrene board

[0071] <![CDATA[Impact strength (kJ / m 2 )]]> Example 1 16.53 Example 2 13.78 Example 5 15.01

[0072] Test Example 2

[0073] The oxygen index of the flame retardant polystyrene board was measured according to the standard GB / T 2406.2-2009 "Determination of combustion behavior of plastics by oxygen index method Part 2: Room temperature test". Ten groups were tested in parallel, and the average value was calculated. The results are shown in Table 2.

[0074] Table 2. Oxygen index test results of polystyrene board

[0075] Initial oxygen index (%) Oxygen index after boiling water for 36 hours (%) Example 1 37.25 37.06 Example 2 34.50 31.85 Example 3 35.71 33.28 Example 4 36.00 35.02 Example 5 36.30 35.61

[0076] By comparing the above embodiments, it can be seen that the flame retardant polystyrene board of Example 1 has the best flame retardant performance, impact strength and stable performance. This is because the modified flame retardant used in Example 1 first uses a combination of polyethylene glycol and sodium polystyrene sulfonate as a dispersant to uniformly disperse the hydrophobic powder flame retardant melamine cyanurate in the aqueous phase, which is conducive to the smooth progress of subsequent modification, and then sequentially modified by polymethacryloyloxyethyl trimethylammonium chloride and aqueous polyaspartic acid ester resin, thereby forming a polyelectrolyte layer and an aqueous polyurea layer on the surface of the hydrophobic powder flame retardant. The aqueous polyaspartic acid ester containing hydrophilic groups such as polyether groups and amino groups is more hydrophilic than the hydrophobic powder flame retardant, and can reduce The surface energy is lowered to reduce the air adsorbed on the powder surface, which increases the packing density of the powder. At the same time, the water-based polyurea layer and the polyelectrolyte cooperate with each other through hydrogen bonds and intermolecular forces, effectively realizing the uniform wrapping of the polymer on the surface of the hydrophobic powder flame retardant. Finally, the polyurea layer is cured by L-lysine diisocyanate to form a more stable interface force, making the wrapping layer denser, and further improving the thermal stability and packing density of the hydrophobic powder flame retardant, which helps to improve the processability and flame retardant efficiency of the hydrophobic powder flame retardant. When added to the polystyrene board matrix, the flame retardant effect of the flame retardant can be guaranteed. At the same time, it has better compatibility with the polystyrene board matrix, which can improve the mechanical and other comprehensive properties of the polystyrene board.

[0077] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A flame retardant polystyrene board, characterized in that: Made of the following raw materials: polystyrene, chlorinated polyethylene, phenolic resin, expanded graphite, polyphenylene sulfide fiber, modified flame retardant, foaming agent, compatibilizer, antioxidant, lubricant; The modified flame retardant is prepared by the following method: adding polyethylene glycol and sodium polystyrene sulfonate into water and mixing them evenly, then adding melamine cyanurate and stirring to obtain a dispersion X; adding magnesium chloride and polymethacryloyloxyethyl trimethyl ammonium chloride into the dispersion X and continuing to stir, then adding an aqueous polyaspartic acid ester resin aqueous dispersion and heating and stirring to obtain a treatment liquid Y; adding L-lysine diisocyanate aqueous dispersion into the treatment liquid Y for curing, filtering, washing with water, and drying after curing to obtain the modified flame retardant.

2. The flame retardant polystyrene board according to claim 1, characterized in that: The invention is made of the following raw materials: 70-100 parts by weight of polystyrene, 5-15 parts by weight of chlorinated polyethylene, 2-8 parts by weight of phenolic resin, 8-12 parts by weight of expanded graphite, 8-12 parts by weight of polyphenylene sulfide fiber, 10-15 parts by weight of modified flame retardant, 5-10 parts by weight of foaming agent, 1-3 parts by weight of compatibilizer, 0.5-1.5 parts by weight of antioxidant and 1-2 parts by weight of lubricant.

3. The flame retardant polystyrene board according to claim 1, characterized in that: The foaming agent is any one of butane foaming agent, pentane foaming agent and pentafluoropropane foaming agent.

4. The flame retardant polystyrene board according to claim 1, characterized in that: The compatibilizer is SEBS-g-MAH.

5. The flame retardant polystyrene board according to claim 1, characterized in that: The lubricant is any one of calcium stearate, polyethylene wax and silicone powder.

6. The flame retardant polystyrene board according to claim 1, characterized in that: The antioxidant is any one of antioxidant 1010, antioxidant 2246, and antioxidant 1076.

7. The method for preparing a flame retardant polystyrene board according to any one of claims 1 to 6, characterized in that: The following steps are involved: Polystyrene, chlorinated polyethylene, phenolic resin and compatibilizer are weighed according to the formula and mixed in an open mill to obtain a blend; then the blend is evenly mixed with expanded graphite, polyphenylene sulfide fiber, modified flame retardant, antioxidant and lubricant, and then melt-mixed in a twin-screw extruder, extruded and pelletized to obtain polystyrene board particles; the polystyrene board particles are mixed with a foaming agent and then placed in an extruder for extrusion molding and dried to obtain the flame-retardant polystyrene board.

8. The method for preparing the flame retardant polystyrene board according to claim 7, characterized in that: The process conditions of the twin-screw extruder are: the temperature range of each zone is 200-240°C, and the main engine speed is 100-300r / min.

Citation Information

Patent Citations

  • Manufacturing method of inorganic modified polystyrene board

    CN104016711B

  • A kind of modified polystyrene board and preparation method thereof

    CN104151730B

  • Fireproof GPES rigid foam composite plastic heat-insulating board and preparation method thereof

    CN108676268A

  • Macromolecular synergistic flame retardant and preparation method thereof