A method for producing a ferrite core

By adjusting the material proportion and production steps, the ferrite core is easily broken and unsuitable moisture content is solved, high-quality finished product production is achieved, and the density and stability of the magnetic core are ensured.

CN117995542BActive Publication Date: 2024-11-12XUYI OU GE ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311837892.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-11-12
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

The ferrite core is prone to breaking or cracking during the production process, and the unsuitable moisture content leads to the quality of the finished product.

Method used

A production method is adopted, including preparation, stirring, press forming, sintering detection, deburring and detection steps, and by adjusting the proportion of materials such as iron oxide, zinc oxide, trimanium tetraoxide, etc., polymer porous composite fillers and bonding are used. The agent controls moisture content and pressure, removes surface burrs and detects bubble generation to ensure finished product quality.

Benefits of technology

It effectively reduces the possibility of fracture of the ferrite core, controls moisture content, improves the density and appearance quality of the finished product, and ensures the stability and efficient production of the finished product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117995542B_ABST
    Figure CN117995542B_ABST
Patent Text Reader

Abstract

The invention discloses a production method of a ferrite core, comprising the following steps: S1. preparing materials: preparing 20-45 parts of iron oxide, 10-35 parts of zinc oxide, 5-28 parts of copper oxide, 10-32 parts of manganese tetraoxide, 5-10 parts of ferroferric oxide, 2-10 parts of additives, 3-15 parts of adhesives, 5-20 parts of carbon fibers and 2-12 parts of additional materials; S2. stirring materials: putting iron oxide, zinc oxide, copper oxide, manganese tetraoxide and ferroferric oxide into a mixing device In the process, a plurality of materials are stirred and mixed together, and then an additive, an adhesive, carbon fiber and an additive are added and stirred to obtain a base material. The iron oxide and manganese tetraoxide and other materials of the present invention are mixed as the matrix of the ferrite core. The additive is a polymer porous composite filler. The polymer porous composite filler has a large porosity ratio and can greatly reduce the possibility of fracture of the ferrite core after molding. The added adhesive polyethylene and the like can make the production material condense, thereby improving the structural compactness of the ferrite core.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ferrite core production, and in particular to a production method of a ferrite core. Background Art

[0002] Ferrite core is a kind of high-frequency magnetic material, mainly used for high-frequency transformers, high-frequency magnetic rings, etc., to increase magnetic permeability and improve inductance quality factor. It is used in transformers and is usually called manganese-zinc ferrite. Ferrite core is an important magnetic material and is widely used in the fields of electronics and electricity.

[0003] For example, a ferrite core with authorization announcement number CN105702422A includes an E-type ferrite core body, wherein the E-type ferrite core body includes a base, a first side column on the left side of the base, a second side column on the right side of the base, and a middle column on the base between the first side column and the second side column.

[0004] During the production process of ferrite cores, if the structure of the ferrite cores is not reasonably adjusted, the possibility of the ferrite cores breaking after production and molding will increase. If the moisture content of the ferrite cores is too low or too high, it will easily cause cracks in the finished ferrite cores or cause the ferrite core materials to stick to the mold. Therefore, it is urgent to design a ferrite core production method to solve the above problems. Summary of the invention

[0005] The object of the present invention is to provide a method for producing a ferrite core to solve the above-mentioned deficiencies in the prior art.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A method for producing a ferrite core comprises the following steps:

[0008] S1. Prepare materials: prepare 20-45 parts of iron oxide, 10-35 parts of zinc oxide, 5-28 parts of copper oxide, 10-32 parts of manganese tetraoxide, 5-10 parts of ferroferric oxide, 2-10 parts of additives, 3-15 parts of adhesives, 5-20 parts of carbon fibers and 2-12 parts of added materials;

[0009] S2. Stirring: Put iron oxide, zinc oxide, copper oxide, manganese tetraoxide and ferromanganese tetraoxide into a mixing device, stir and mix the various materials together, then add filler, adhesive, carbon fiber and additional material and stir to obtain the base material. The porosity ratio formula of the filler is:

[0010]

[0011] In the formula, K is the porosity ratio of the filler,

[0012] e is the porosity of the filler;

[0013] S3. Compression molding: The base material is placed in a pressing mold, and a certain pressure is applied to the base material using an extrusion device so that the base material is formed in the mold;

[0014] S4. Sintering test: After the temperature in the sintering equipment is raised to a certain level, the pressed material is placed in the sintering equipment to be sintered into a sintered part and cooled to room temperature;

[0015] S5. Moisture content detection: The detection contact of the moisture detector contacts the sintered part, and the moisture detector detects the moisture content of the sintered part. The formula for detecting the moisture content of the sintered part is:

[0016]

[0017] In the formula, H is the moisture content after sintering,

[0018] The sintered wet weight is n,

[0019] The sintered dry weight is z;

[0020] S6 Deburring: Prepare a deburring tool, and remove the burrs on the surface of the sintered part obtained in S4 by a deburring tool to obtain a ferrite core production material;

[0021] S7. Detection: Wipe the surface of the ferrite core production material with kerosene or alcohol, check whether there are bubbles on the surface of the ferrite core production material, and then heat the ferrite core to stabilize the temperature and detect the temperature after stabilization.

[0022] Preferably, in S2, the proportion of the iron oxide mixture is 20%, the proportion of zinc oxide is 10%, the proportion of copper oxide is 5-10%, the proportion of manganese tetraoxide is 5-12%, and the proportion of ferrosoferric oxide is 7-18%.

[0023] Preferably, in S2, the ratio of the filler, adhesive, carbon fiber and added material is 4:6:8:3, and the filler is one of a polymer porous composite filler or a composite granular material.

[0024] Preferably, in S2, the adhesive is one of paraffin and polyethylene, and the carbon fiber is graphite fiber material.

[0025] Preferably, in S2, the added material is polyester fiber, and the rotation speed of stirring and mixing the various materials is 120 rpm.

[0026] Preferably, in S3, the pressure applied by the extrusion equipment is 40-100 MPa, and in S4, the temperature in the sintering equipment is pre-sintered to 120°C.

[0027] Preferably, in S4, the pressed material is placed in a sintering device and fired at a temperature of 800-1200° C., and the sintered part is cooled at a rate of 100-380° C. / hour.

[0028] Preferably, in said S4, the temperature of cooling to room temperature is 23°C, and in said S5, the moisture content of the sintered part is detected and controlled within a range of 0.5%-3.5%.

[0029] Preferably, in S6, when the sintered part is processed by a deburring tool, the deburring is performed at a rotation speed of 300 revolutions per minute.

[0030] Preferably, in S7, the temperature is stabilized after heating for 4 hours, and if the temperature after stabilization is detected to be no more than 110° C., the product can be continuously produced.

[0031] In the above technical scheme, the present invention provides a method for producing a ferrite core, by setting iron oxide, filler and adhesive, iron oxide and manganese tetraoxide and other materials are mixed as the matrix of the ferrite core, the filler is a polymer porous composite filler, the polymer porous composite filler has a large porosity, which can greatly reduce the possibility of the ferrite core breaking after molding, and the added adhesive polyethylene and the like can make the production material condense, thereby improving the structural compactness of the ferrite core; by setting the pressing molding and moisture content detection, the moisture content of the sintered part is detected and controlled within a certain range, and the lower moisture content is difficult to cause the molding material to stick to the mold, so that the ferrite core production and molding are rapid, and the molding material can be obtained after extrusion; by setting the deburring and detection, the burrs on the surface of the sintered part can be removed by using the deburring tool to improve the appearance quality, and then detect whether bubbles are generated on the surface of the ferrite core production material to ensure the production yield of the ferrite core. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can also be obtained based on these drawings.

[0033] Figure 1 A schematic diagram of the steps of a production method provided for a ferrite core production method embodiment of the present invention Figure 1 .

[0034] Figure 2 A schematic diagram of the steps of a production method provided for a ferrite core production method embodiment of the present invention Figure 2 .

[0035] Figure 3 A schematic diagram of the steps of a production method provided for a ferrite core production method embodiment of the present invention Figure 3 . DETAILED DESCRIPTION

[0036] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be further described in detail below with reference to the accompanying drawings.

[0037] Embodiment 1

[0038] like Figure 1-3 As shown, a method for producing a ferrite core provided by an embodiment of the present invention comprises the following steps:

[0039] S1. Prepare materials: prepare 20 parts of iron oxide, 15 parts of zinc oxide, 8 parts of copper oxide, 15 parts of manganese tetraoxide, 5 parts of ferroferric oxide, 6 parts of additives, 9 parts of adhesive, 12 parts of carbon fiber and 10 parts of added material;

[0040] S2. Stirring: Put iron oxide, zinc oxide, copper oxide, manganese tetraoxide and ferroferric oxide into a mixing device, the proportion of iron oxide is 20%, the proportion of zinc oxide is 10%, the proportion of copper oxide is 7%, the proportion of manganese tetraoxide is 8%, and the proportion of ferroferric oxide is 12%, and the various materials are stirred and mixed together, and then the filler, adhesive, carbon fiber and the added material are added and stirred. The ratio of the filler, adhesive, carbon fiber and the added material is 4:6:8:3, the filler is a composite granular material, the adhesive is paraffin, the carbon fiber is a graphite fiber material, and the added material is polyester fiber. The speed of stirring and mixing the various materials is 120 rpm to obtain the base material. The porosity formula of the filler is:

[0041]

[0042] In the formula, K is the porosity ratio of the filler,

[0043] e is the porosity of the filler;

[0044] S3 compression molding: the base material is placed in a pressing mold, and a certain pressure is applied to the base material by an extrusion device. The pressure applied by the extrusion device is 80MPa, so that the base material is formed in the mold;

[0045] S4. Sintering test: The temperature in the sintering equipment is increased to 120°C for pre-sintering, and the pressed material is placed in the sintering equipment for sintering to obtain a sintered part and cooled to room temperature. The pressed material is placed in the sintering equipment for sintering at a temperature of 900°C, and the sintered part is cooled at a cooling rate of 290°C / hour, and the temperature cooled to room temperature is 23°C;

[0046] S5. Moisture content detection: The detection contact of the moisture detector contacts the sintered part, and the moisture detector detects the moisture content of the sintered part. The formula for detecting the moisture content of the sintered part is:

[0047]

[0048] In the formula, H is the moisture content after sintering,

[0049] The sintered wet weight is n,

[0050] The sintered dry weight is z,

[0051] The moisture content of the sintered parts is controlled at 2.5%;

[0052] S6 Deburring: Prepare a deburring tool, S4 prepared sintered part by deburring tool to remove burrs on the surface, the deburring speed is 300 rpm, to obtain a ferrite core production material;

[0053] S7. Inspection: Wipe the surface of the ferrite core production material with kerosene or alcohol, check whether there are bubbles on the surface of the ferrite core production material, and then heat the ferrite core. After heating for 4 hours, stabilize the temperature and check the temperature after stabilization. If the temperature after stabilization does not exceed 110℃, it can be used as a finished product for continuous production.

[0054] Embodiment 2

[0055] A method for producing a ferrite core provided by an embodiment of the present invention comprises the following steps:

[0056] S1. Prepare materials: prepare 25 parts of iron oxide, 18 parts of zinc oxide, 18 parts of copper oxide, 20 parts of manganese tetraoxide, 7 parts of ferroferric oxide, 7 parts of additives, 9 parts of adhesive, 5 parts of carbon fiber and 6 parts of added material;

[0057] S2. Stirring: Put iron oxide, zinc oxide, copper oxide, manganese tetraoxide and ferroferric oxide into a mixing device, the proportion of iron oxide is 20%, the proportion of zinc oxide is 10%, the proportion of copper oxide is 5%, the proportion of manganese tetraoxide is 10%, and the proportion of ferroferric oxide is 9%, and the various materials are stirred and mixed together, and then the filler, adhesive, carbon fiber and the added material are added and stirred. The ratio of the filler, adhesive, carbon fiber and the added material is 4:6:8:3. The filler is a porous composite filler of a polymer, the adhesive is polyethylene, the carbon fiber is a graphite fiber material, and the added material is a polyester fiber. The speed of stirring and mixing the various materials is 120 rpm to obtain a base material. The porosity formula of the filler is:

[0058]

[0059] In the formula, K is the porosity ratio of the filler,

[0060] e is the porosity of the filler;

[0061] S3 compression molding: the base material is placed in a pressing mold, and a certain pressure is applied to the base material by an extrusion device. The pressure applied by the extrusion device is 80MPa, so that the base material is formed in the mold;

[0062] S4. Sintering test: The temperature in the sintering equipment is increased to 120°C for pre-sintering, and the pressed material is placed in the sintering equipment for sintering to obtain a sintered part and cooled to room temperature. The pressed material is placed in the sintering equipment for sintering at a temperature of 1200°C, and the sintered part is cooled at a cooling rate of 300°C / hour, and the temperature cooled to room temperature is 23°C;

[0063] S5. Moisture content detection: The detection contact of the moisture detector contacts the sintered part, and the moisture detector detects the moisture content of the sintered part. The formula for detecting the moisture content of the sintered part is:

[0064]

[0065] In the formula, H is the moisture content after sintering,

[0066] The sintered wet weight is n,

[0067] The sintered dry weight is z,

[0068] The moisture content of the sintered parts is controlled at 1.5%;

[0069] S6 Deburring: Prepare a deburring tool, S4 prepared sintered part by deburring tool to remove burrs on the surface, the deburring speed is 300 rpm, to obtain a ferrite core production material;

[0070] S7. Inspection: Wipe the surface of the ferrite core production material with kerosene or alcohol, check whether there are bubbles on the surface of the ferrite core production material, and then heat the ferrite core. After heating for 4 hours, stabilize the temperature and check the temperature after stabilization. If the temperature after stabilization does not exceed 110℃, it can be used as a finished product for continuous production.

[0071] Embodiment 3

[0072] A method for producing a ferrite core provided by an embodiment of the present invention comprises the following steps:

[0073] S1. Prepare materials: prepare 35 parts of iron oxide, 25 parts of zinc oxide, 16 parts of copper oxide, 19 parts of manganese tetraoxide, 7 parts of ferroferric oxide, 8 parts of additives, 5 parts of adhesive, 10 parts of carbon fiber and 7 parts of added material;

[0074] S2. Stirring: Put iron oxide, zinc oxide, copper oxide, manganese tetraoxide and ferroferric oxide into a mixing device, the proportion of iron oxide is 20%, the proportion of zinc oxide is 10%, the proportion of copper oxide is 8%, the proportion of manganese tetraoxide is 8%, and the proportion of ferroferric oxide is 12%, and the various materials are stirred and mixed together, and then the filler, adhesive, carbon fiber and the added material are added and stirred, the ratio of the filler, adhesive, carbon fiber and the added material is 4:6:8:3, the filler is a porous composite filler of a polymer, the adhesive is one of the paraffins, the carbon fiber is a graphite fiber material, and the added material is a polyester fiber. The speed of stirring and mixing the various materials is 120 rpm to obtain a base material. The porosity formula of the filler is:

[0075]

[0076] In the formula, K is the porosity ratio of the filler,

[0077] e is the porosity of the filler;

[0078] S3 compression molding: the base material is placed in a pressing mold, and a certain pressure is applied to the base material by an extrusion device. The pressure applied by the extrusion device is 70MPa, so that the base material is formed in the mold;

[0079] S4. Sintering test: The temperature in the sintering equipment is increased to 120°C for pre-sintering, and the pressed material is placed in the sintering equipment for sintering to obtain a sintered part and cooled to room temperature. The pressed material is placed in the sintering equipment for sintering at a temperature of 950°C, and the sintered part is cooled at a cooling rate of 200°C / hour, and the temperature cooled to room temperature is 23°C;

[0080] S5. Moisture content detection: The detection contact of the moisture detector contacts the sintered part, and the moisture detector detects the moisture content of the sintered part. The formula for detecting the moisture content of the sintered part is:

[0081]

[0082] In the formula, H is the moisture content after sintering,

[0083] The sintered wet weight is n,

[0084] The sintered dry weight is z,

[0085] The moisture content of the sintered parts was controlled at 2.6%;

[0086] S6 Deburring: Prepare a deburring tool, S4 prepared sintered part by deburring tool to remove burrs on the surface, the deburring speed is 300 rpm, to obtain a ferrite core production material;

[0087] S7. Inspection: Wipe the surface of the ferrite core production material with kerosene or alcohol, check whether there are bubbles on the surface of the ferrite core production material, and then heat the ferrite core. After heating for 4 hours, stabilize the temperature and check the temperature after stabilization. If the temperature after stabilization does not exceed 110℃, it can be used as a finished product for continuous production.

[0088] Working principle: The material composition and proportion used in Example 1, Example 2 and Example 3 are different, and the temperature, duration and pressure value of the production method are different, the filling materials used are different, and the other parameters are consistent. By conducting experimental comparison on the final ferrite core finished product, the above three groups of embodiments are obtained through experiments and preparation, and the effect in Example 2 is the best. In Example 2, after preparing the materials, iron oxide, zinc oxide, copper oxide, manganese tetraoxide, iron tetraoxide, filling materials, adhesives, carbon fibers and added materials are mixed and stirred. The filling materials used are polymer porous composite fillers. When the polymer porous composite fillers are prepared, the porosity of the polymer porous composite fillers is large, so that the fracture resistance of the ferrite core is reduced. By using polyethylene, graphite fiber materials and polymer The ester fiber condenses the production material tightly, and the production material is then placed in a pressing mold for extrusion. The moisture content of the sintered part is detected and controlled at 1.5%. Too much moisture content will cause the molding material to stick to the mold. When the moisture content is controlled within a certain range, the molding material can be prevented from sticking to the mold or cracking. The molding material can be obtained after extrusion. The molding material is placed in a sintering device and fired to a certain temperature, and then cooled to obtain a sintered part. The sintered part is tested with a moisture detector, and the burrs on the surface of the sintered part are removed with a deburring tool. Then, kerosene or alcohol is used to wipe the surface of the ferrite core production material to check whether bubbles are generated. If bubbles are not generated, the ferrite core has a high density and no fractures. The ferrite core is then heated and the temperature of the ferrite core is detected after it stabilizes, and it can finally be produced as a finished product.

[0089] The above description is only by way of illustration of certain exemplary embodiments of the present invention. It is undoubted that those skilled in the art can modify the described embodiments in various ways without departing from the spirit and scope of the present invention. Therefore, the above drawings and descriptions are illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.

Claims

1. A method for producing a ferrite core, It is characterized in that The following steps are involved: S1. Prepare materials: prepare 20-45 parts of iron oxide, 10-35 parts of zinc oxide, 5-28 parts of copper oxide, 10-32 parts of manganese tetraoxide, 5-10 parts of ferroferric oxide, 2-10 parts of additives, 3-15 parts of adhesives, 5-20 parts of carbon fibers and 2-12 parts of added materials; S2. Stirring: Put iron oxide, zinc oxide, copper oxide, manganese tetraoxide and ferromanganese tetraoxide into a mixing device, stir and mix the various materials together, then add filler, adhesive, carbon fiber and additional material and stir to obtain the base material. The porosity ratio formula of the filler is: , In the formula, K is the porosity ratio of the filler, e is the porosity of the filler, In S2, the ratio of the filler, adhesive, carbon fiber and added material is 4:6:8:3, and the filler is a polymer porous composite filler; S3. Compression molding: The base material is placed in a pressing mold, and a certain pressure is applied to the base material using an extrusion device so that the base material is formed in the mold; S4. Sintering test: After the temperature in the sintering equipment is raised to a certain level, the pressed material is placed in the sintering equipment to be sintered into a sintered part and cooled to room temperature; S5. Moisture detection: The detection contact of the moisture detector contacts the sintered part, and the moisture detector detects the moisture content of the sintered part. The formula for detecting the moisture content of the sintered part is: , In the formula, H is the moisture content after sintering, The sintered wet weight is n, The sintered dry weight is z; S6 Deburring: Prepare a deburring tool, and remove the burrs on the surface of the sintered part obtained in S4 by a deburring tool to obtain a ferrite core production material; S7. Inspection: Wipe the surface of the ferrite core production material with kerosene or alcohol to check whether there are bubbles on the surface of the ferrite core production material, and then heat the ferrite core to stabilize the temperature and detect the temperature after stabilization; In the S2, the proportion of iron oxide is 20%, the proportion of zinc oxide is 10%, the proportion of copper oxide is 5-10%, the proportion of manganese tetraoxide is 5-12%, and the proportion of ferroferric oxide is 7-18%. In the S2, the added material is polyester fiber, and the rotation speed of stirring and mixing multiple materials is 120 rpm. In the S3, the pressure applied by the extrusion equipment is 40-100MPa. In the S4, the temperature in the sintering equipment is pre-burned to 120°C. In the S4, the pressed molding material is placed in the sintering equipment at a firing temperature of 800-1200°C, and the cooling rate of the sintered part is 100-380°C / hour. In the S4, the temperature cooled to room temperature is 23°C. In the S5, the moisture content of the sintered part is detected and controlled at 0.5%-3.5%.

2. The method for producing a ferrite core according to claim 1, It is characterized in that In S2, the adhesive is one of paraffin and polyethylene, and the carbon fiber is graphite fiber material.

3. The method for producing a ferrite core according to claim 1, It is characterized in that In the above S6, when the sintered part is processed by the deburring tool, the deburring is performed at a rotation speed of 300 rpm.

4. The method for producing a ferrite core according to claim 1, It is characterized in that In S7, the temperature is stabilized after heating for 4 hours, and the temperature after stabilization is detected to be no more than 110° C., that is, the finished product is continuously produced.