Aluminum alloy welding wire for fusion welding of 6XXX series aluminum alloy extruded profiles, preparation method and application thereof

By using Al3 (ScxZr1-x) particles formed by Zr and Sc in aluminum alloy welding wire to refine the weld structure, the problem of liquefied cracks in joints after melting and welding of 6XXX aluminum alloy materials is solved, and the weld strength and mechanical properties are improved. It provides a foundation for its application in the field of engineering.

CN118002980BActive Publication Date: 2024-12-03CHINALCO MATERIALS APPL RES INST CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410427043.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-10
Publication Date
2024-12-03
Estimated Expiration
2044-04-10

AI Technical Summary

Technical Problem

The joints of 6XXX series aluminum alloy materials are prone to liquefaction cracks after melting and welding, resulting in poor mechanical properties.

Method used

Aluminum alloy welding wires with specific components include 0~0.2% Si, 0~0.2% Fe, 0.2% Mn, 5.8~6.8% Mg, 0~0.04% Ti, 0.1~0.12% Zr , 0.25~0.35% Sc, the balance is Al and inevitable impurities. Through the synergistic action of Zr and Sc, Al3 (ScxZr1-x) particles are formed as heterogeneous nucleation particles, refine the weld structure, and reduce Mg and Si. Elements penetrate along the crystal, reducing the tendency of liquefied cracks.

Benefits of technology

Effectively reduce the tendency of weld liquefied cracks, improve weld strength, and improve the mechanical properties of joints, laying the foundation for the engineering application of 6XXX series extruded profiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118002980B_ABST
    Figure CN118002980B_ABST
Patent Text Reader

Abstract

The present invention provides an aluminum alloy welding wire for fusion welding of 6XXX series aluminum alloy extruded profiles. The components of the aluminum alloy welding wire include, by mass percentage, 0-0.2% Si, 0-0.2% Fe, 0-0.05% Cu, 0.2-0.3% Mn, 5.8-6.8% Mg, 0-0.04% Ti, 0.1-0.12% Zr, 0.25-0.35% Sc, and the remainder is Al and unavoidable impurities, each unavoidable impurity is less than 0.05%, and the total impurities are less than 0.15%. The aluminum alloy welding wire of the present invention has a specific aluminum alloy component ratio, and contains Sc and Zr at the same time, which can effectively refine the weld structure. When applied to the fusion welding of 6XXX series aluminum alloy extruded profiles, it can effectively reduce the tendency of weld liquefaction cracks and improve the weld strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of high-strength aluminum alloy welding wire manufacturing, and in particular to an aluminum alloy welding wire used for fusion welding of 6XXX series aluminum alloy extruded profiles, and a preparation method and application thereof. Background Art

[0002] 6XXX series aluminum alloy is an Al-Mg-Si series aluminum alloy that can be heat-treated and strengthened. It has good ductility and is the preferred material for manufacturing large extruded profiles. It is often used in the fields of ships, rail transportation, etc.

[0003] In the prior art, fusion welding is often used to assemble 6XXX series aluminum alloy as a load-bearing structure. However, due to the influence of aluminum profile extrusion process, the surface of 6XXX series aluminum alloy material will have the problem of coarse grains. At the same time, 6XXX series aluminum alloy has a large amount of second phases at the grain boundary and in the grain. After being applied to fusion welding, the obtained joint is prone to liquefaction cracks in the partial melting zone, and the mechanical properties of the joint are poor. Summary of the invention

[0004] The main purpose of the present invention is to provide an aluminum alloy welding wire for fusion welding of 6XXX series aluminum alloy extruded profiles, a preparation method and application thereof, so as to solve the problem in the prior art that liquefaction cracks are easily generated in the molten zone of the joint during fusion welding of 6XXX series aluminum alloy materials, resulting in poor mechanical properties of the joint.

[0005] In order to achieve the above object, according to one aspect of the present invention, an aluminum alloy welding wire for fusion welding of 6XXX series aluminum alloy extruded profiles is provided. In terms of mass percentage, the composition of the aluminum alloy welding wire includes: 0-0.2% Si, 0-0.2% Fe, 0-0.05% Cu, 0.2-0.3% Mn, 5.8-6.8% Mg, 0-0.04% Ti, 0.1-0.12% Zr, 0.25-0.35% Sc, and the balance is Al and unavoidable impurities, each unavoidable impurity is less than 0.05%, and the total impurities are less than 0.15%.

[0006] Furthermore, calculated by mass percentage, the composition of the aluminum alloy welding wire includes: 0~0.06% Si, 0~0.12% Fe, 0~0.05% Cu, 0.2~0.3% Mn, 6~6.6% Mg, 0~0.04% Ti, 0.1~0.12% Zr, 0.3~0.35% Sc, and the remainder is Al and unavoidable impurities, each unavoidable impurity is <0.05%, and the total impurities are <0.15%.

[0007] Furthermore, in the composition of the aluminum alloy welding wire, the mass ratio of Zr to Sc is 1:(2~3).

[0008] According to another aspect of the present invention, a method for preparing an aluminum alloy welding wire for fusion welding of 6XXX series aluminum alloy extruded profiles is provided. The method comprises the following steps: step S1, mixing the raw materials with reference to the composition of the aluminum alloy welding wire, and then performing melting and casting to obtain an aluminum alloy cast rod; step S2, homogenizing and annealing the aluminum alloy cast rod, and then extruding to obtain a first wire rod; step S3, alternately drawing and intermediate annealing the first wire rod to obtain a second wire rod; step S4, sequentially rough scraping, wire drawing, and fine scraping the second wire rod to obtain a third wire rod; step S5, cleaning the third wire rod to obtain an aluminum alloy welding wire.

[0009] Furthermore, in step S1, during the melting and casting, the liquid online hydrogen content is controlled to be ≤0.12 ml / 100g.

[0010] Furthermore, in step S2, the temperature of the homogenization annealing is 440-470° C., and the time is 8-24 hours; and / or the diameter of the first wire is 10-11 mm.

[0011] Furthermore, in step S2, the temperature of the homogenization annealing is 450-470° C., and the time is 8-12 hours.

[0012] Furthermore, in step S3, the diameter reduction in each drawing pass is 0.72-0.8 mm.

[0013] Furthermore, in step S3, the intermediate annealing temperature is 350-400° C., and the time is 2-3 hours; and the diameter of the second wire is 2.05-2.25 mm.

[0014] Further, in step S4, the scraping speed of rough scraping is 3.5~4.5m / s; the diameter reduction of rough scraping is 0.1~0.2mm; and / or the diameter reduction of wire drawing is 0.45~0.8mm; and / or the diameter reduction of fine scraping is 0.1~0.12mm.

[0015] Furthermore, in step S5, the cleaning temperature is 50-60°C.

[0016] Furthermore, in step S5, the diameter of the aluminum alloy welding wire is 1.18-1.6 mm.

[0017] According to another aspect of the present invention, a method for welding aluminum alloy is provided, which uses a 6XXX series aluminum alloy extruded profile with surface coarse grains as a base material and performs fusion welding with the above-mentioned aluminum alloy welding wire.

[0018] Furthermore, the atmosphere of the fusion welding is 99.99% argon.

[0019] According to another aspect of the present invention, there is provided a welding joint obtained by using the above welding method, the welding joint having no liquefaction cracks.

[0020] The aluminum alloy welding wire of the present invention has a specific aluminum alloy composition ratio and contains Sc and Zr at the same time. During the solidification process of the molten pool of the molten welding, Zr, Sc and Al cooperate with each other to form Al3 (Sc x Zr 1-x ) particles can act as heterogeneous nucleation particles to effectively refine the weld structure, transform the coarse columnar crystals in the weld fusion zone into equiaxed crystals, reduce the intercrystalline penetration of Mg and Si elements, and effectively reduce the precipitation of low-melting-point MgSi (MgSiCu) eutectic phases between grain boundaries, thereby reducing the tendency of liquid cracks to form in the partial melting zone of the fusion weld joint under welding heat input, which is beneficial to improve the mechanical strength of the joint.

[0021] The aluminum alloy welding wire of the present invention has good weldability. When used for fusion welding of 6XXX series aluminum alloy extruded profiles, it can effectively reduce the tendency of weld liquefaction cracks and improve the weld strength, thus laying a foundation for the promotion and application of 6XXX series extruded profiles in the engineering field. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0023] Figure 1 A surface morphology diagram of a 6XXX series extruded profile according to an embodiment of the present invention is shown;

[0024] Figure 2 The microstructure diagram of the weld of the aluminum alloy welding wire of Example 1 of the present invention applied to 6XXX series extruded profiles is shown;

[0025] Figure 3 The microstructure diagram of the weld of the aluminum alloy welding wire of Example 2 of the present invention applied to 6XXX series extruded profiles is shown;

[0026] Figure 4 The microstructure diagram of the weld of the aluminum alloy welding wire of Comparative Example 1 of the present invention applied to 6XXX series extruded profiles is shown;

[0027] Figure 5 The microstructure diagram of the weld of the aluminum alloy welding wire of Comparative Example 2 of the present invention applied to 6XXX series extruded profiles is shown;

[0028] Figure 6 The microstructure diagram of the weld of the aluminum alloy welding wire of Comparative Example 3 of the present invention applied to 6XXX series extruded profiles is shown; and

[0029] Figure 7 The microstructure diagram of the partial melting zone of the welding seam of the welding wire of Comparative Example 1 of the present invention is shown;

[0030] The above drawings include the following reference numerals:

[0031] 1. Melting zone part 1; 2. Melting zone part 2. DETAILED DESCRIPTION

[0032] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0033] As described in the background of the present invention, there is a problem in the prior art that liquefaction cracks are generated in the partial melting zone of the joint of the 6XXX series aluminum alloy material, resulting in poor mechanical properties of the joint. In order to solve the above problem, in a typical embodiment of the present invention, an aluminum alloy welding wire is provided, and the composition of the aluminum alloy welding wire includes, by mass percentage: 0~0.2% Si, 0~0.2% Fe, 0~0.05% Cu, 0.2~0.3% Mn, 5.8~6.8% Mg, 0~0.04% Ti, 0.1~0.12% Zr, 0.25~0.35% Sc, and the balance is Al and unavoidable impurities, each unavoidable impurity is less than 0.05%, and the total impurities are less than 0.15%.

[0034] Mg can improve the mechanical strength of welded joints through solid solution strengthening. If the mass percentage of Mg in the welding wire is lower than 5.8%, when the welding wire is used for melting welding of 6XXX series aluminum alloy materials, the obtained joint will have less Mg elements dissolved in the α-Al matrix, and the joint strength will be weakened; if the mass percentage of Mg is higher than 6.8%, the addition of too much Mg element will increase the cost of the welding wire. At the same time, too much Mg will easily absorb hydrogen during the melting and casting process, resulting in excessive hydrogen content in the liquid line, even higher than 0.12ml / 100g.

[0035] The aluminum alloy welding wire of the present invention has a specific aluminum alloy composition ratio and contains Sc and Zr at the same time. During the solidification process of the molten pool of the molten welding, Zr, Sc and Al cooperate with each other to form Al3 (Sc x Zr 1-x ) (such as Al3(Sc 0.5 Zr 0.5 )) particles can act as heterogeneous nucleation particles to effectively refine the weld structure, transform the coarse columnar crystals in the weld fusion zone into equiaxed crystals, reduce the intercrystalline penetration of Mg and Si elements, and effectively reduce the precipitation of low-melting-point MgSi (MgSiCu) eutectic phases between grain boundaries, thereby reducing the tendency of liquid cracks to form in the partial melting zone of the fusion weld joint under welding heat input, which is beneficial to improve the mechanical strength of the joint.

[0036] In a preferred embodiment, the composition of the aluminum alloy welding wire includes, by mass percentage, 0-0.06% Si, 0-0.12% Fe, 0-0.05% Cu, 0.2-0.3% Mn, 6-6.6% Mg, 0-0.04% Ti, 0.1-0.12% Zr, 0.3-0.35% Sc, and the balance is Al and unavoidable impurities, each unavoidable impurity is less than 0.05%, and the total impurities are less than 0.15%. Under the above conditions, the precipitation of MgSi (MgSiCu) eutectic phase between grain boundaries can be further reduced, which is more conducive to reducing the liquefaction cracks caused by the partial melting zone of the fusion welding joint during welding heat input.

[0037] Regarding the mass ratio of Zr and Sc in the aluminum alloy welding wire, in order to reduce production costs, in the prior art, Sc and Zr can be added to the welding wire composition in a mass ratio of Zr and Sc of 1:1. x Zr 1-x ) phase, nearly 50% of Sc atoms will be replaced by Zr atoms. In order to be more conducive to the Al3(Sc x Zr 1-x ) particle formation, which is further conducive to the refinement of the weld structure. In a preferred embodiment, the mass ratio of Zr to Sc in the composition of the aluminum alloy welding wire is 1: (2-3). Under the above conditions, it is more conducive to obtaining Al3 (Sc x Zr 1-x ), more effectively reducing the precipitation of MgSi (MgSiCu) eutectic phase caused by the intercrystalline penetration of Mg and Si elements.

[0038] In another typical embodiment of the present invention, a method for preparing an aluminum alloy welding wire for fusion welding of 6XXX series aluminum alloy extruded profiles is also provided, comprising the following steps: step S1, mixing the raw materials with reference to the composition of the aluminum alloy welding wire, and then performing melt casting to obtain an aluminum alloy cast rod; step S2, homogenizing and annealing the aluminum alloy cast rod, and then extruding it to obtain a first wire rod; step S3, alternately drawing and intermediate annealing the first wire rod to obtain a second wire rod; step S4, sequentially rough scraping, drawing, and fine scraping the second wire rod to obtain a third wire rod; step S5, cleaning the third wire rod to obtain an aluminum alloy welding wire.

[0039] The present invention first mixes and melts the raw materials of the aluminum alloy welding wire to obtain a cast rod. Next, the cast rod is homogenized and annealed to eliminate dendrite segregation in the cast rod and make the structure of each element homogenized. Then, the annealed cast rod is extruded, and alternately drawn and intermediate annealed to obtain a second wire. Extrusion and drawing cooperate with each other, which is conducive to eliminating cast rod segregation and reducing structural shrinkage. Drawing and intermediate annealing are alternately performed to soften the cast rod after drawing, which is convenient for alternate drawing operations on the cast rod.

[0040] Next, the second wire is subjected to rough scraping, wire drawing, and fine scraping in sequence to obtain the third wire. The process of wire drawing between two wire scrapings can effectively improve the surface quality of the wire and ensure continuous and stable wire feeding of the welding wire. Finally, the third wire is cleaned, which can further improve the surface quality of the aluminum alloy welding wire without reducing the diameter of the wire. It should be noted that the alternating drawing and intermediate annealing in the present invention refers to the cycle of "single drawing-single intermediate annealing-single drawing-single intermediate annealing".

[0041] The preparation method of the present invention can realize processing and production on a conventional production line without modifying the production line, and the cost is controllable. The prepared aluminum alloy welding wire grains have good weldability. When the welding wire of the present invention is used for fusion welding of 6XXX series extruded profiles, the tendency of weld liquefaction cracks can be effectively reduced, and the weld strength can be improved, laying a foundation for the subsequent promotion and application of 6XXX series extruded profiles.

[0042] In order to further reduce defects such as pores and microporosity of aluminum alloy cast rods, thereby further improving the quality of welding wires, in a preferred embodiment, in step S1, during melt casting, the liquid online hydrogen content is controlled to be ≤0.12 ml / 100g.

[0043] In the prior art, the homogenization annealing system is divided into short-time annealing and long-time annealing. In order to effectively reduce energy consumption and welding wire cost, the present invention particularly selects a homogenization annealing system with shorter time consumption. In a preferred embodiment, in step S2, the temperature of homogenization annealing is 440~470℃, and the time is 8~24h. Under the above conditions, the process takes less time, consumes less energy, and the effect of uniform organization is better, and the mechanical properties of the joint obtained when used for welding are further increased. If the temperature of homogenization annealing is too high or the time is too long, the energy consumption is large and the cost is high. If the temperature of homogenization annealing is too low or the time is too short, the segregation of cast rods cannot be effectively eliminated, which is not conducive to uniform organization. In order to further shorten the process time consumption and reduce energy consumption, in a preferred embodiment, in step S2, the temperature of homogenization annealing is 450~470℃, and the time is 8~12h. Under the above conditions, the prepared welding wire organization is still uniform. Preferably, the diameter of the first wire is 10~11 mm.

[0044] In a preferred embodiment, in step S3, the diameter reduction of each drawing pass is 0.72~0.8 mm. On the basis of the diameter reduction of each drawing pass, the drawing passes can be set in combination with the actual situation, which is understandable to those skilled in the art and will not be repeated here. If the diameter reduction of each drawing pass is too small, there will be too many drawing passes, and the processing process will be more complicated, time-consuming and costly. If the diameter reduction of each drawing pass is too much under the premise of the same total diameter reduction, the wire is easy to break during the drawing process, and the surface quality of the wire is poor, with many pits and cracks, and it is easy to jump the arc when applied to 6XXX series extruded profiles for melting welding. In a preferred embodiment, the diameter of the second wire is 2.05~2.25 mm.

[0045] In order to facilitate the processing of wires, in a preferred embodiment, the intermediate annealing temperature is 350-400°C and the time is 2-3 hours. If the annealing temperature is too low or the time is too short, the annealing is not thorough, resulting in a harder wire, which is not conducive to the subsequent drawing process. If the annealing temperature is too high or the time is too long, the wire surface will be significantly oxidized, the wire oxide scale will be too thick, resulting in more impurities during welding, poor mechanical properties, and not suitable for application in fusion welding.

[0046] For the purpose of more conducive to continuous and stable wire feeding, in a preferred embodiment, in step S4, the scraping speed of rough scraping is 3.5~4.5m / s. If the scraping speed of rough scraping is too fast, the surface quality of the wire is poor, and if the rough scraping speed is too slow, the production efficiency is too low. In a preferred embodiment, the diameter reduction of rough scraping is 0.1~0.2mm; and / or the diameter reduction of wire drawing is 0.45~0.8mm; and / or the diameter reduction of fine scraping is 0.1~0.12mm. In a preferred embodiment, in step S5, the diameter of the aluminum alloy welding wire is 1.18~1.6mm.

[0047] In a preferred embodiment, in step S5, the cleaning temperature is 50-60°C. If the cleaning temperature is too low, the oil stains on the surface of the welding wire are not easy to clean. In a preferred embodiment, step S5 also includes the steps of drying and coiling the cleaned third wire. Under the above conditions, it is more conducive to the storage and transportation of aluminum alloy welding wire.

[0048] In another typical embodiment of the present invention, a method for welding aluminum alloy is provided, which uses a 6XXX series aluminum alloy extruded profile with surface coarse grains as a base material and performs fusion welding with the above-mentioned aluminum alloy welding wire.

[0049] In a preferred embodiment, the atmosphere of the fusion welding is 99.99% argon. Under the above conditions, the welding effect of the fusion welding is better and the joint quality is better.

[0050] In another typical embodiment of the present invention, there is also provided a welding joint obtained by using the above welding method, wherein the welding joint has no liquefaction cracks and has high strength and good quality.

[0051] The present invention enables the aluminum alloy welding wire to have better weldability from the perspectives of limiting the composition of the aluminum alloy welding wire, limiting the preparation method of the welding wire and optimizing the welding process. When applied to the fusion welding of 6XXX series aluminum alloy extruded profiles, the generation of joint liquefaction cracks is effectively reduced, the weld strength is increased, and the mechanical properties of the joint are significantly improved, laying a foundation for the promotion and application of 6XXX series extruded profiles in the engineering field.

[0052] Typically, but not limiting, the aluminum alloy welding wire for fusion welding of 6XXX series aluminum alloy extruded profiles is composed of the following components, measured by mass percentage: Si 0, 0.01%, 0.02%, 0.04%, 0.06%, 0.08%, 0.1%, 0.12%, 0.14%, 0.15%, 0.16%, 0.18%, 0.2% or a range consisting of any two of them; Fe 0, 0.01%, 0.02%, 0.04%, 0.06%, 0.08%, 0.1%, 0.12%, 0.14%, 0.15%, 0.16%, 0.18%, 0.2% or a range consisting of any two of them; Cu 0, 0.01%, 0.02%, 0.03%, 0.04%, 0.05% or a range consisting of any two of them; Mn 0.2%, 0.22%, 0.24%, 0.26%, 0.28%, 0.3% or a range consisting of any two of them; Mg 5.8%, 6%, 6.2%, 6.4%, 6.6%, 6.8% or a range consisting of any two of them; Ti 0%, 0.01%, 0.02%, 0.03%, 0.04% or a range consisting of any two of them; Zr 0.1%, 0.11%, 0.12% or a range consisting of any two of them; Sc 0.25%, 0.27%, 0.29%, 0.3%, 0.31%, 0.33%, 0.35% or a range consisting of any two of them; the balance is Al and unavoidable impurities, each unavoidable impurity is <0.05%, and the total impurities are <0.15%.

[0053] Typically but not limiting, the mass ratio of Zr to Sc in the composition of the aluminum alloy welding wire is 1:2, 1:2.2, 1:2.4, 1:2.6, 1:2.8, 1:3 or a range consisting of any two of them.

[0054] Typically but not limitatively, in step S2, the temperature of the homogenization treatment is 440°C, 445°C, 450°C, 455°C, 460°C, 465°C, 470°C or a range consisting of any two of them; and the time is 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h or a range consisting of any two of them.

[0055] Typically but not limiting, in step S3, the diameter reduction in each drawing pass is 0.72 mm, 0.74 mm, 0.76 mm, 0.78 mm, 0.8 mm or a range consisting of any two of them.

[0056] Typically but not limiting, in step S3, the intermediate annealing temperature is 350°C, 360°C, 370°C, 380°C, 390°C, 400°C, and the time is 2h, 2.2h, 2.4h, 2.6h, 2.8h, 3h or a range consisting of any two of them.

[0057] Typically but not limiting, in step S5, the cleaning temperature is 50°C, 52°C, 54°C, 56°C, 58°C, 60°C or a range consisting of any two of them.

[0058] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0059] Example 1

[0060] Step S1, referring to the composition of the aluminum alloy welding wire, mixing the raw materials, and then performing melting and casting, controlling the liquid online hydrogen content to 0.11 ml / 100 g, to obtain a φ140 mm aluminum alloy cast rod;

[0061] Step S2, performing homogenization annealing on the aluminum alloy cast rod at 455° C. for 10 h; and then extruding the cast rod into a first wire rod of φ10.18 mm;

[0062] Step S3, the first wire is alternately subjected to 11 drawing passes and 11 intermediate annealing passes to obtain a φ2.15 mm second wire; the diameter reduction in each drawing pass is 0.73 mm, the intermediate annealing system is 375° C., and the holding time is 2.5 hours;

[0063] Step S4, then, using a flat die to roughly scrape the second wire, the scraping speed is 4m / s, and the φ2.15mm aluminum alloy wire is scraped to φ2mm; then, a small amount of processing is used to water-box wire drawing the φ2mm wire to φ1.3mm; the φ1.3mm wire is finely scraped using a flat die, and the fine scraping reduction is 0.11mm, to obtain a third wire of φ1.19mm;

[0064] Step S5, ultrasonically clean the third wire material with a diameter of 1.19 mm, and control the water temperature at 55° C. Thereafter, the third wire material is dried and finally coiled to obtain an aluminum alloy welding wire.

[0065] Step S6, under the protection of 99.99% argon, a 6XXX extruded profile with surface coarse grains is used as a base material and melt-welded with an aluminum alloy welding wire, and no liquefaction cracks are generated in the welded joint.

[0066] Examples 2 to 8

[0067] The only difference from Example 1 is:

[0068] The composition of aluminum alloy welding wire is different, see Table 1 for details.

[0069] Example 9

[0070] Step S1, referring to the composition of the aluminum alloy welding wire in Example 1, mixing the raw materials, and then performing melting and casting, controlling the liquid online hydrogen content to 0.10 ml / 100g, to obtain a φ140 mm aluminum alloy cast rod;

[0071] Step S2, homogenizing and annealing the aluminum alloy cast rod at 440° C. for 9 hours; and then extruding the cast rod into a first wire rod of φ10.15 mm;

[0072] Step S3, the first wire is alternately drawn 10 times and intermediate annealed 10 times to obtain a φ2.15 mm second wire; the diameter reduction of each drawing pass is 0.8 mm, the intermediate annealing system is 350° C., and the holding time is 3 hours;

[0073] Step S4, then, using a flat die to roughly scrape the second wire, the scraping speed is 4m / s, the rough scraping diameter reduction is 0.1mm, and the φ2.15mm aluminum alloy wire is scraped to φ2.05mm; then, a small amount of processing is used to water-box wire drawing the φ2.05mm wire, and the wire drawing diameter reduction is 0.45mm; wire drawing to φ1.6mm; the φ1.6mm wire is finely scraped using a flat die, and the fine scraping diameter reduction is 0.1mm, to obtain a φ1.5mm third wire;

[0074] Step S5, ultrasonically clean the third wire of φ1.5 mm, and control the water temperature at 60° C. Thereafter, dry the third wire, and finally coil it to obtain an aluminum alloy welding wire;

[0075] Step S6, under the protection of 99.99% argon, a 6XXX extruded profile with surface coarse grains is used as a base material and melt-welded with an aluminum alloy welding wire, and no liquefaction cracks are generated in the welded joint.

[0076] Example 10

[0077] The only difference from Example 1 is:

[0078] In step S2, the homogenization annealing temperature is 450° C. and the time is 12 h.

[0079] Comparative Example 1

[0080] The only difference from Example 1 is:

[0081] The aluminum alloy welding wire raw material does not contain Sc, and the mass percentage of Mg is 5%.

[0082] Comparative Example 2

[0083] The only difference from Example 1 is:

[0084] The composition of aluminum alloy welding wire is different, see Table 1 for details.

[0085] Comparative Example 3

[0086] The only difference from Example 1 is:

[0087] The aluminum alloy welding wire raw material does not contain Sc, and the mass percentage of Mg is 6.3%.

[0088] Comparative Example 4

[0089] The only difference from Example 1 is:

[0090] Aluminum alloy welding wire raw materials do not contain Zr.

[0091] Comparative Example 5

[0092] The only difference from Example 1 is:

[0093] The number of drawing passes is 7, and the diameter reduction in each drawing pass is 1.0 mm.

[0094] Comparative Example 6

[0095] The only difference from Example 1 is:

[0096] Fine scraping process is not included.

[0097] Comparative Example 7

[0098] The only difference from Example 1 is:

[0099] The cleaning temperature is 20°C.

[0100] The raw material compositions of the aluminum alloy welding wires of the above embodiments and comparative examples are shown in Table 1; the mechanical properties of the welded joints formed by the aluminum alloy welding wires of the above embodiments and comparative examples on 6XXX series extruded profiles are shown in Table 2.

[0101] Surface morphology of 6XXX series extruded profiles Figure 1 ; The aluminum alloy welding wire of Example 1 is applied to the weld microstructure of 6XXX series extruded profiles. Figure 2 ; The aluminum alloy welding wire of Example 2 is applied to the weld microstructure of the 6XXX series extruded profile. Figure 3 Comparative Example 1 of aluminum alloy welding wire applied to 6XXX series extruded profile weld microstructure diagram see Figure 4 Comparative Example 2 of aluminum alloy welding wire applied to 6XXX series extruded profile weld microstructure diagram see Figure 5 Comparative Example 3 of aluminum alloy welding wire applied to 6XXX series extruded profile weld microstructure diagram see Figure 6 The microstructure diagram of the partial melting zone of the welding seam of the welding wire of comparative example 1 is shown in Figure 7 , element content analysis was performed on melting zone part 1 and melting zone part 2, and the spectrum labels are shown in Table 3.

[0102] Test method:

[0103] Element content test: refer to 》to test.

[0104] Tensile test: Refer to GB / T 2651-2023 Destructive test of metal material welds - transverse tensile test, 》to test.

[0105] Table 1

[0106]

[0107] Table 2

[0108]

[0109] Table 3

[0110]

[0111] As can be seen from the above, compared with the comparative example, the embodiments of the present invention control the specific aluminum alloy composition ratio and contain Sc and Zr at the same time. During the solidification process of the molten pool of fusion welding, Zr, Sc and Al cooperate with each other to form Al3 (Sc x Zr 1-x) particles act as heterogeneous nucleation particles, effectively refining the weld structure, transforming the coarse columnar crystals in the weld fusion zone into equiaxed crystals, reducing the penetration of Mg and Si elements along the crystals, and effectively reducing the precipitation of low-melting-point MgSi (MgSiCu) eutectic phases between grain boundaries, thereby reducing the tendency of liquefaction cracks to occur in the partial molten zone of the fusion weld joint under welding heat input, thereby facilitating the improvement of the mechanical strength of the joint. The aluminum alloy welding wire of the present invention has good weldability, and when used in fusion welding of 6XXX series aluminum alloy extruded profiles, it can effectively reduce the tendency of liquefaction cracks in the weld and improve the weld strength. In addition, it can be seen that when all process parameters are within the preferred range of the present invention, the mechanical strength of the welding wire is higher.

[0112] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An aluminum alloy welding wire for fusion welding of 6XXX series aluminum alloy extruded profiles, characterized in that: The 6XXX series aluminum alloy extruded profile has surface coarse grains, and the composition of the aluminum alloy welding wire is composed of the following components by mass percentage: 0-0.06% Si, 0-0.12% Fe, 0-0.05% Cu, 0.2-0.3% Mn, 6-6.6% Mg, 0-0.04% Ti, 0.1-0.12% Zr, 0.3-0.35% Sc, the balance being Al and unavoidable impurities, each of the unavoidable impurities being <0.05%, and the total impurities being <0.15%; and the mass ratio of Zr to Sc being 1:(2.6-3); The method for preparing the aluminum alloy welding wire comprises the following steps: Step S1, referring to the composition of the aluminum alloy welding wire, mixing the raw materials, and then performing melting and casting to obtain an aluminum alloy cast rod; Step S2, homogenizing and annealing the aluminum alloy cast rod, and then extruding it to obtain a first wire rod; Step S3, alternately drawing and intermediate annealing the first wire to obtain a second wire; Step S4, sequentially rough-scraping, wire-drawing, and fine-scraping the second wire to obtain a third wire; Step S5, cleaning the third wire material to obtain the aluminum alloy welding wire; In step S2, the homogenization annealing time is 8 to 24 hours; In the step S3, the diameter reduction of each drawing pass is 0.72-0.8 mm; the number of drawing passes is 11; The intermediate annealing temperature is 350-400°C; In the step S4, the scraping speed of the rough scraping is 3.5-4.5 m / s; the diameter reduction of the rough scraping is 0.1-0.2 mm; and the diameter reduction of the fine scraping is 0.1-0.12 mm.

2. The method for preparing the aluminum alloy welding wire for fusion welding of 6XXX series aluminum alloy extruded profiles according to claim 1, characterized in that: The following steps are involved: Step S1, referring to the composition of the aluminum alloy welding wire, mixing the raw materials, and then performing melting and casting to obtain an aluminum alloy cast rod; Step S2, homogenizing and annealing the aluminum alloy cast rod, and then extruding it to obtain a first wire rod; Step S3, alternately drawing and intermediate annealing the first wire to obtain a second wire; Step S4, sequentially rough-scraping, wire-drawing, and fine-scraping the second wire to obtain a third wire; Step S5, cleaning the third wire material to obtain the aluminum alloy welding wire.

3. The preparation method according to claim 2, characterized in that: In the step S1, during the melting and casting, the liquid online hydrogen content is controlled to be ≤0.12 ml / 100 g.

4. The preparation method according to claim 2, characterized in that: In the step S2, The homogenization annealing temperature is 440-470° C. and the time is 8-24 hours; and / or The diameter of the first wire is 10-11 mm.

5. The preparation method according to claim 2, characterized in that: In the step S2, The homogenization annealing temperature is 450-470° C. and the time is 8-12 hours.

6. The preparation method according to claim 2, characterized in that: In the step S3, The diameter reduction in each drawing pass is 0.72 to 0.8 mm.

7. The preparation method according to claim 2, characterized in that: In the step S3, The intermediate annealing temperature is 350-400°C and the time is 2-3h; The diameter of the second wire is 2.05-2.25 mm.

8. The preparation method according to claim 2, characterized in that: In the step S4, The scraping speed of the rough scraping is 3.5-4.5 m / s; The diameter reduction of the rough scraping is 0.1 to 0.2 mm; and / or The wire drawing has a diameter reduction of 0.45 to 0.8 mm; and / or The diameter reduction of the fine scraping is 0.1 to 0.12 mm.

9. The preparation method according to claim 2, characterized in that: In the step S5, The cleaning temperature is 50-60°C.

10. The preparation method according to claim 2, characterized in that: In the step S5, The diameter of the aluminum alloy welding wire is 1.18-1.6 mm.

11. A method for welding aluminum alloy, characterized in that: A 6XXX series aluminum alloy extruded profile with surface coarse grains is used as a base material and is melt-welded with the aluminum alloy welding wire described in claim 1.

12. The welding method according to claim 11, characterized in that: The atmosphere of the fusion welding is 99.99% argon.

13. A welding joint, characterized in that: The welding method according to claim 11 or 12 is used to obtain a weld joint free of liquefaction cracks.