A method for preparing non-stoichiometric multi-component carbide solid solution ceramic with high carbon vacancy content
Through the methods of high-energy ball milling and solid-phase sintering, the problems of low density and oxygen pollution of multi-component carbide ceramic materials with high carbon vacancy content are solved, high density and mechanical properties are improved, the process flow is simplified and the cost is reduced. cost.
Patent Information
- Application Number
- CN202410151111.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-02
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-02-02
AI Technical Summary
Existing non-stoichiometric multi-component carbide solid solution ceramic materials with high carbon vacancy content have problems such as low density, many impurities, complex process flow and low degree of controllability. In particular, they are prone to oxygen contamination and cold during the sintering process. Welding problem.
The high-energy ball milling method is used to fully mix the transition metal carbide powder and the hydride powder to form a carbide and hydride composite powder with high sintering activity, and obtain a multi-component carbide with a high carbon vacancy content through a solid-phase sintering reaction. Solid solution ceramics, the carbon content is controlled to avoid oxygen contamination, and sintered in an argon or vacuum environment to increase the density and purity of the material.
It effectively improves the density and mechanical properties of the material, lowers the sintering temperature, reduces oxygen pollution, improves the purity and production controllability of the material, and greatly reduces the cost. The density exceeds 97%, and the room temperature hardness and modulus are significantly improved. .
Smart Images

Figure CN118005400B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of special ceramic materials, and in particular relates to a method for preparing a non-stoichiometric ratio multi-component carbide solid solution ceramic with a high carbon vacancy content. Background Art
[0002] Transition metal carbide ceramic materials have excellent properties such as high melting point, high hardness, and good chemical stability, so they are considered to have broad application prospects in extreme environments. Transition metal carbides are usually non-stoichiometric, and the carbon vacancies of some transition metal carbides can even reach 50%. Studies on multi-component carbide solid solution ceramics have shown that changes in carbon content can significantly affect the physical phase, structure, sintering activity, mechanical properties and thermal properties of multi-component carbide ceramics. The reduction in carbon content can promote the atomic diffusion and single-phase formation of multi-component carbide ceramics, which is beneficial to reduce the sintering temperature and increase the density of the material. In addition, the carbon content will also have a significant effect on the mechanical properties of multi-component carbide ceramics. The presence of an appropriate amount of carbon vacancies can improve the mechanical properties of multi-component carbide ceramics. In current reports, non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content generally have problems such as low density, many impurities, or complex process flow and low controllability. Therefore, it is very necessary to provide a new method for preparing non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content. Summary of the invention
[0003] The purpose of the present invention is to solve the problems of low density, high impurities or complex process flow with low controllability, cold welding and easy oxygen contamination in the existing non-stoichiometric multi-component carbide solid solution ceramic powders with high carbon vacancy content, and to provide a preparation method of non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content.
[0004] A method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content is specifically completed by the following steps:
[0005] 1. Weigh the required powder:
[0006] ①, weighing one of niobium carbide, tantalum carbide and hafnium carbide powders or weighing two or three of niobium carbide, tantalum carbide and hafnium carbide powders in equal molar ratio to obtain metal carbide powder;
[0007] ②, weigh titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, and the molar numbers of titanium carbide and zirconium carbide powders are equal, to obtain mixed powder I;
[0008] The molar ratio of the titanium hydride and titanium carbide described in step 1② to the metal carbide powder weighed in step 1① is where 0.5 < x < 1.0, n is the sum of the types of metal carbides weighed in Step 1① and Step 1②, 1 ≤ n ≤ 3, and n is an integer;
[0009] II. Mixing:
[0010] The metal carbide powder weighed in Step 1① and the mixed powder I weighed in Step 1② are preliminarily mixed, and then high-energy ball milling is carried out in an argon atmosphere or a vacuum environment to make the powder fully and evenly mixed, and the powder is crushed to reduce the particle size of the powder to improve its solid solution and sintering activity, obtaining mixed powder II;
[0011] III. Sintering:
[0012] The mixed powder II obtained in Step 2 is placed in a mold for sintering to obtain a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content.
[0013] The chemical formula of the non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content is (TiZrM)C x , (TiZrM1M2)C x , (TiZrM1M2M3)C x , where 0.5 < x < 1.0, M is one of Nb, Ta, and Hf; M1M2 are two of Nb, Ta, and Hf; M1M2M3 are Nb, Ta, and Hf.
[0014] The present invention has the following beneficial effects:
[0015] I. The present invention firstly proposes a preparation method of a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content. Through high-energy ball milling, the transition metal carbide powder and the hydride powder are fully mixed to form a carbide and hydride composite powder with high sintering activity, and then by means of solid-phase sintering, a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content is obtained through reaction sintering; high-energy ball milling can fully mix the carbide and the hydride, ensure the uniformity of element distribution, and improve the sintering activity by crushing particles, which can effectively improve the density of the material and reduce the sintering temperature; selecting hydride powder to regulate the carbon content can effectively avoid oxygen pollution, solve the problems of oxidation and cold welding that are prone to occur during the high-energy ball milling of metal powder, and at the same time can realize the adjustable and controllable carbon vacancy content, broadening the material design space;
[0016] II. The non-stoichiometric multi-component carbide solid solution ceramic prepared by applying the present invention can effectively reduce free carbon and residual oxygen, reduce the sintering preparation temperature, improve the density of the material and refine the grains;
[0017] 3. The process flow of the present invention is simple, which greatly reduces the production cost of non-stoichiometric multi-component carbide solid solution ceramic materials with high carbon vacancy content, and significantly improves the controllability in the production and preparation process, reduces the possibility of oxygen contamination, and the oxygen content is less than 0.3%, ensuring the purity of non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content. The non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content prepared by the present invention have a relative density of >97%, a room temperature hardness of 25 to 35 GPa, a modulus of 400 to 500 GPa, and a fracture toughness of 3 to 5 MPa·m 1 / 2 .
[0018] The invention can obtain a non-stoichiometric ratio multi-component carbide solid solution ceramic with high carbon vacancy content. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The chemical formula prepared in Example 1 is (TiZrNb)C 0.8 XRD patterns of non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0020] Figure 2 The chemical formula prepared in Example 1 is (TiZrNb)C 0.8 SEM image of non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0021] Figure 3 The chemical formula prepared in Example 1 is (TiZrNb)C 0.8 In-situ SEM image of the elemental surface distribution of non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0022] Figure 4 for Figure 3 Ti element distribution diagram in;
[0023] Figure 5 for Figure 3 Zr element distribution diagram in;
[0024] Figure 6 for Figure 3 Nb element distribution diagram in. DETAILED DESCRIPTION
[0025] The following examples are intended to further illustrate the present invention, but should not be construed as limiting the present invention. Without departing from the essence of the present invention, modifications and substitutions made to the methods, steps or conditions of the present invention are within the scope of the present invention.
[0026] Embodiment 1: A preparation method of a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content is completed according to the following steps:
[0027] I. Weigh the required powders:
[0028] ① Weigh one of niobium carbide, tantalum carbide and hafnium carbide powders, or weigh two or three of niobium carbide, tantalum carbide and hafnium carbide powders according to an equimolar ratio to obtain a metal carbide powder;
[0029] ② Weigh titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders, where the molar amounts of titanium hydride and zirconium hydride powders are equal, and the molar amounts of titanium carbide and zirconium carbide powders are equal, to obtain a mixed powder I;
[0030] The molar ratio of titanium hydride, titanium carbide in step ② of step I to the metal carbide powder weighed in step ① of step I is where 0.5 < x < 1.0, n is the sum of the types of metal carbides weighed in step ① and step ② of step I, 1 ≤ n ≤ 3, and n is an integer;
[0031] II. Mixing:
[0032] Preliminarily mix the metal carbide powder weighed in step ① of step I with the mixed powder I weighed in step ② of step I, and then perform high-energy ball milling in an argon atmosphere or a vacuum environment to make the powders fully and evenly mixed, and crush the powders to reduce the powder particle size to improve their solid solution and sintering activities, obtaining a mixed powder II;
[0033] III. Sintering:
[0034] Place the mixed powder II obtained in step II into a mold for sintering to obtain a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content.
[0035] Embodiment 2: The difference between this embodiment and Embodiment 1 is that the chemical formulas of the niobium carbide, tantalum carbide and hafnium carbide powders described in step ① of step I are NbC, TaC and HfC respectively, and the purity of each is > 99.0 wt.%. Other steps are the same as those in Embodiment 1.
[0036] Embodiment 3: The difference between this embodiment and one of Embodiment 1 or 2 is that the chemical formulas of the titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders described in step ② of step I are TiC, ZrC, TiH₂ and ZrH₂ respectively, and the purity of each is > 99.0 wt.%. Other steps are the same as those in Embodiment 1 or 2.
[0037] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the ball-to-material ratio of the high-energy ball mill described in step 2 is (10-50):1, the rotation speed of the high-energy ball mill is 100 r / min-700 r / min, the time of the high-energy ball mill is 5h-40h, and the material of the ball mill jar and the grinding ball is cemented carbide. The other steps are the same as those of specific embodiments 1 to 3.
[0038] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that the sintering method described in step 3 is spark plasma sintering. The other steps are the same as those of specific embodiments 1 to 4.
[0039] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the spark plasma sintering process described in step 3 is: heating from room temperature to 1800-2400°C, keeping at 1800-2400°C for 1min-30min, then cooling to room temperature, the heating rate is 10°C / min-200°C / min, the cooling rate is 50°C / min-200°C / min, and the pressure is maintained at 10-100MPa during the sintering process. The other steps are the same as those of specific embodiments 1 to 5.
[0040] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that the sintering method described in step 3 is hot pressing sintering. The other steps are the same as those of specific embodiments 1 to 6.
[0041] Specific embodiment eight: This embodiment differs from specific embodiments one to seven in that the hot pressing sintering process described in step three is: heating from room temperature to 1800-2400°C, keeping at 1800-2400°C for 1min-120min, then cooling to room temperature, heating rate of 5°C / min-30°C / min, cooling rate of 5°C / min-50°C / min, and keeping pressure of 10MPa-100MPa during sintering. Other steps are the same as specific embodiments one to seven.
[0042] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: in the sintering process in step 3, an inert gas needs to be continuously introduced to form a protective atmosphere or maintain a vacuum state; the inert gas is argon, helium or krypton; the vacuum state is <20 Pa. The other steps are the same as those of specific embodiments 1 to 8.
[0043] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that the chemical formula of the non-stoichiometric multi-component carbide solid solution ceramic with high carbon vacancy content described in step 3 is (TiZrM)C x , (TiZrM1M2)C x, (TiZrM1M2M3)C x , where 0.5 < x < 1.0, M is one of Nb, Ta, and Hf; M1M2 is two of Nb, Ta, and Hf; M1M2M3 is Nb, Ta, and Hf. Other steps are the same as those in Embodiments 1 to 9.
[0044] The beneficial effects of the present invention are verified by the following examples:
[0045] Example 1: A preparation method of a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content is specifically completed according to the following steps:
[0046] 1. Design a non-stoichiometric multi-component carbide solid solution ceramic with the chemical formula (TiZrNb)C 0.8 and weigh the required powders:
[0047] ①. Weigh niobium carbide to obtain a metal carbide powder;
[0048] ②. Weigh titanium carbide, zirconium carbide, titanium hydride, and zirconium hydride powders, where the molar amounts of titanium hydride and zirconium hydride powders are equal, and the molar amounts of titanium carbide and zirconium carbide powders are equal, to obtain a mixed powder I;
[0049] The molar ratio of titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, and niobium carbide described in Step 1② is 3:3:7:7:10;
[0050] The purities of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, and niobium carbide powders described in Step 1 are all > 99.0 wt.%;
[0051] 2. Mixing:
[0052] Preliminarily mix the metal carbide powder weighed in Step 1① with the mixed powder I weighed in Step 1②, and then perform high-energy ball milling in a vacuum environment to make the powders fully and uniformly mixed, and crush the powders to reduce the powder particle size to improve their solid solution and sintering activities, obtaining a mixed powder II;
[0053] The process parameters of the high-energy ball milling described in Step 2 are: the ball-to-powder ratio is 10:1, the rotation speed of the ball mill is 300 r / min, the ball milling time is 5 h, and the materials of the ball mill tank and grinding balls are both cemented carbide;
[0054] 3. Sintering:
[0055] Place the mixed powder II obtained in Step 2 in a mold and perform spark plasma sintering under argon protection to obtain a non-stoichiometric multi-component carbide solid solution ceramic with the chemical formula (TiZrNb)C 0.8 and a high carbon vacancy content;
[0056] The spark plasma sintering process described in step three is: heating from room temperature to 2200°C, keeping at 2200°C for 10 minutes, and then cooling to room temperature, with a heating rate of 50°C / min and a cooling rate of 100°C / min. The pressure is maintained at 30MPa during the sintering process.
[0057] Example 1 The chemical formula of the prepared 0.8 The non-stoichiometric multi-component carbide solid solution ceramic with high carbon vacancy content has uniform distribution of metal elements, a grain size of 18.3μm, a density of 99.6%, a hardness of 33.3GPa, a three-point bending strength of 470MPa, an elastic modulus of 430GPa, and a fracture toughness of 3.82MPa·m 1 / 2 .
[0058] Figure 1 The chemical formula prepared in Example 1 is (TiZrNb)C 0.8 XRD patterns of non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0059] from Figure 1 It can be seen that the chemical formula prepared in Example 1 is (TiZrNb)C 0.8 The non-stoichiometric multi-component carbide solid solution ceramic with high carbon vacancy content is a single phase without any impurities and second phases, which proves that the single-phase (TiZrNb)C 0.8 Non-stoichiometric multi-component carbide ceramic materials.
[0060] Figure 2 The chemical formula prepared in Example 1 is (TiZrNb)C 0.8 SEM image of non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0061] from Figure 2 It can be seen that the chemical formula prepared in Example 1 is (TiZrNb)C 0.8 The non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content have high density, relatively uniform grain size distribution, and no abnormal growth phenomenon.
[0062] Figure 3 The chemical formula prepared in Example 1 is (TiZrNb)C 0.8 In-situ SEM image of the elemental surface distribution of non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0063] Figure 4 for Figure 3 Ti element distribution diagram in;
[0064] Figure 5 for Figure 3 Zr element distribution diagram in;
[0065] Figure 6 for Figure 3 Nb element distribution diagram in.
[0066] Figure 3 to Figure 6 It shows that the chemical formula of Example 1 is (TiZrNb)C 0.8 The Ti, Zr and Nb metal elements are evenly distributed in the non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content, without obvious element segregation, which once again proves that the single-phase (TiZrNb)C 0.8 Non-stoichiometric multi-component carbide ceramic materials.
[0067] Embodiment 2: A method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content is specifically completed by the following steps:
[0068] 1. The designed chemical formula is (TiZrNb)C 0.6 Non-stoichiometric multi-component carbide solid solution ceramics, weigh the required powder:
[0069] ①. Weigh niobium carbide to obtain metal carbide powder;
[0070] ②, weigh titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, and the molar numbers of titanium carbide and zirconium carbide powders are equal, to obtain mixed powder I;
[0071] The molar ratio of titanium hydride, zirconium hydride, titanium carbide, zirconium carbide and niobium carbide described in step 1② is 3:3:2:2:5;
[0072] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide and niobium carbide powders in step 1 is > 99.0wt.%;
[0073] 2. Mixing:
[0074] The metal carbide powder weighed in step 1① is preliminarily mixed with the mixed powder I weighed in step 1②, and then high-energy ball milling is performed in a vacuum environment to make the powders fully and evenly mixed, and the powders are crushed to reduce the particle size of the powders to improve their solid solution and sintering activity, thereby obtaining mixed powder II;
[0075] The process parameters of the high-energy ball milling in step 2 are: the ball-to-material ratio is 30:1, the speed of the ball mill is 700 r / min, the ball milling time is 20 h, and the materials of the ball mill and the grinding balls are both cemented carbide;
[0076] 3. Sintering:
[0077] The mixed powder II obtained in step 2 is placed in a mold and spark plasma sintered under argon protection to obtain a (TiZrNb)C 0.6 Non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0078] The spark plasma sintering process described in step three is: heating from room temperature to 2200°C, keeping at 2200°C for 5 minutes, and then cooling to room temperature, with a heating rate of 100°C / min, a cooling rate of 200°C / min, and maintaining a pressure of 70MPa during the sintering process.
[0079] Example 2 The chemical formula of the prepared product is (TiZrNb)C 0.6 The non-stoichiometric multi-component carbide solid solution ceramic with high carbon vacancy content has uniform distribution of metal elements, a density of 99.4%, a hardness of 31.7GPa, a three-point bending strength of 430MPa, an elastic modulus of 400GPa, and a fracture toughness of 3.92MPa·m 1 / 2 .
[0080] Embodiment 3: A method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content is specifically completed by the following steps:
[0081] 1. The designed chemical formula is (TiZrNb)C 0.9 Non-stoichiometric multi-component carbide solid solution ceramics, weigh the required powder:
[0082] ①. Weigh niobium carbide to obtain metal carbide powder;
[0083] ②, weigh titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, and the molar numbers of titanium carbide and zirconium carbide powders are equal, to obtain mixed powder I;
[0084] The molar ratio of titanium hydride, zirconium hydride, titanium carbide, zirconium carbide and niobium carbide described in step 1② is 3:3:17:17:20;
[0085] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide and niobium carbide powders in step 1 is > 99.0wt.%;
[0086] 2. Mixing:
[0087] The metal carbide powder weighed in step 1① is preliminarily mixed with the mixed powder I weighed in step 1②, and then high-energy ball milling is performed in a vacuum environment to make the powders fully and evenly mixed, and the powders are crushed to reduce the particle size of the powders to improve their solid solution and sintering activity, thereby obtaining mixed powder II;
[0088] The process parameters of the high-energy ball milling in step 2 are: a ball-to-material ratio of 50:1, a ball mill speed of 500 r / min, a ball milling time of 40 h, and the materials of the ball milling jar and the grinding balls are both cemented carbide;
[0089] 3. Sintering:
[0090] The mixed powder II obtained in step 2 is placed in a mold and spark plasma sintered under vacuum conditions to obtain a (TiZrNb)C 0.9 Non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0091] The spark plasma sintering process described in step three is: heating from room temperature to 2400°C, keeping at 2400°C for 30 minutes, and then cooling to room temperature, with a heating rate of 150°C / min and a cooling rate of 50°C / min. The pressure is maintained at 100MPa during the sintering process.
[0092] Example 3 The chemical formula of the prepared product is (TiZrNb)C 0.9 The non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content have uniform distribution of metal elements, a density of 99.8%, a hardness of 34.7GPa, a three-point bending strength of 490MPa, an elastic modulus of 489GPa, and a fracture toughness of 4.72MPa·m 1 / 2 .
[0093] Embodiment 4: A method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content is specifically completed by the following steps:
[0094] 1. The designed chemical formula is (TiZrNbTa)C 0.8 Non-stoichiometric multi-component carbide solid solution ceramics, weigh the required powder:
[0095] ①, weighing niobium carbide and tantalum carbide in equal molar ratio to obtain metal carbide powder;
[0096] ②, weigh titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, and the molar numbers of titanium carbide and zirconium carbide powders are equal, to obtain mixed powder I;
[0097] The molar ratio of titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and tantalum carbide described in step 1② is 2:2:3:3:5:5;
[0098] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and tantalum carbide powders in step 1 is all > 99.0wt.%;
[0099] 2. Mixing:
[0100] The metal carbide powder weighed in step 1① is preliminarily mixed with the mixed powder I weighed in step 1②, and then high-energy ball milling is performed in a vacuum environment to make the powders fully and evenly mixed, and the powders are crushed to reduce the particle size of the powders to improve their solid solution and sintering activity, thereby obtaining mixed powder II;
[0101] The process parameters of the high-energy ball milling in step 2 are: the ball-to-material ratio is 30:1, the speed of the ball mill is 200 r / min, the ball milling time is 10 h, and the materials of the ball mill and the grinding balls are both cemented carbide;
[0102] 3. Sintering:
[0103] The mixed powder II obtained in step 2 is placed in a mold and spark plasma sintered under vacuum conditions to obtain a (TiZrNbTa)C 0.8 Non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0104] The spark plasma sintering process described in step three is: heating from room temperature to 2100°C, keeping at 2100°C for 25 minutes, and then cooling to room temperature, with a heating rate of 50°C / min and a cooling rate of 100°C / min. The pressure is maintained at 75MPa during the sintering process.
[0105] Example 4 The chemical formula of the prepared product is (TiZrNbTa)C 0.8 The non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content have uniform distribution of metal elements, a density of 99.2%, a hardness of 34.1GPa, a three-point bending strength of 477MPa, an elastic modulus of 451GPa, and a fracture toughness of 4.89MPa·m 1 / 2 .
[0106] Embodiment 5: A method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content is specifically completed by the following steps:
[0107] 1. The designed chemical formula is (TiZrNbTa)C 0.8 Non-stoichiometric multi-component carbide solid solution ceramics, weigh the required powder:
[0108] ①, weighing niobium carbide and tantalum carbide in equal molar ratio to obtain metal carbide powder;
[0109] ②, weigh titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, and the molar numbers of titanium carbide and zirconium carbide powders are equal, to obtain mixed powder I;
[0110] The molar ratio of titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and tantalum carbide described in step 1② is 2:2:3:3:5:5;
[0111] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and tantalum carbide powders in step 1 is all > 99.0wt.%;
[0112] 2. Mixing:
[0113] The metal carbide powder weighed in step 1① is preliminarily mixed with the mixed powder I weighed in step 1②, and then high-energy ball milling is performed in a vacuum environment to make the powders fully and evenly mixed, and the powders are crushed to reduce the particle size of the powders to improve their solid solution and sintering activity, thereby obtaining mixed powder II;
[0114] The process parameters of the high-energy ball milling in step 2 are: the ball-to-material ratio is 30:1, the speed of the ball mill is 200 r / min, the ball milling time is 10 h, and the materials of the ball mill and the grinding balls are both cemented carbide;
[0115] 3. Sintering:
[0116] The mixed powder II obtained in step 2 is placed in a mold and hot-pressed and sintered under vacuum to obtain a powder with the chemical formula (TiZrNbTa)C 0.8 Non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0117] The hot pressing sintering process described in step three is: heating from room temperature to 2200°C, keeping at 2200°C for 1 hour, and then cooling to room temperature, with a heating rate of 5°C / min, a cooling rate of 50°C / min, and maintaining a pressure of 75MPa during the sintering process.
[0118] Example 5 The chemical formula of the prepared product is (TiZrNbTa)C 0.8 The non-stoichiometric multi-component carbide solid solution ceramic with high carbon vacancy content has uniform distribution of metal elements, a density of 99.3%, a hardness of 34.6GPa, a three-point bending strength of 467MPa, an elastic modulus of 448GPa, and a fracture toughness of 4.92MPa·m 1 / 2 .
[0119] Example 6: A method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content, which is specifically completed by the following steps:
[0120] 1. The designed chemical formula is (TiZrHfNbTa)C 0.8 Non-stoichiometric multi-component carbide solid solution ceramics, weigh the required powder:
[0121] ①, weighing niobium carbide, tantalum carbide and hafnium carbide in equal molar ratio to obtain metal carbide powder;
[0122] ②, weigh titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, and the molar numbers of titanium carbide and zirconium carbide powders are equal, to obtain mixed powder I;
[0123] The molar ratio of titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide, tantalum carbide and hafnium carbide described in step 1② is 1:1:1:1:2:2:2;
[0124] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide, tantalum carbide and hafnium carbide powders in step 1 is all > 99.0wt.%;
[0125] 2. Mixing:
[0126] The metal carbide powder weighed in step 1① is preliminarily mixed with the mixed powder I weighed in step 1②, and then high-energy ball milling is performed in a vacuum environment to make the powders fully and evenly mixed, and the powders are crushed to reduce the particle size of the powders to improve their solid solution and sintering activity, thereby obtaining mixed powder II;
[0127] The process parameters of the high-energy ball milling in step 2 are: the ball-to-material ratio is 20:1, the speed of the ball mill is 450 r / min, the ball milling time is 25 h, and the materials of the ball mill and the grinding balls are both cemented carbide;
[0128] 3. Sintering:
[0129] The mixed powder II obtained in step 2 is placed in a mold and hot-pressed and sintered under vacuum to obtain a powder with the chemical formula (TiZrHfNbTa)C 0.8 Non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0130] The hot pressing sintering process described in step three is: heating from room temperature to 1800°C, keeping at 1800°C for 2 hours, and then cooling to room temperature, with a heating rate of 20°C / min, a cooling rate of 20°C / min, and a pressure of 30MPa during sintering.
[0131] Example 6 The chemical formula of the prepared product is (TiZrHfNbTa)C 0.8 The non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content have uniform distribution of metal elements, a density of 99.9%, a hardness of 28.6GPa, a three-point bending strength of 427MPa, an elastic modulus of 418GPa, and a fracture toughness of 3.42MPa·m 1 / 2 .
[0132] Embodiment 7: A method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content is specifically completed by the following steps:
[0133] 1. The designed chemical formula is (TiZrHfTa)C 0.8 Non-stoichiometric multi-component carbide solid solution ceramics, weigh the required powder:
[0134] ①, weighing tantalum carbide and hafnium carbide in equal molar ratio to obtain metal carbide powder;
[0135] ②, weigh titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, and the molar numbers of titanium carbide and zirconium carbide powders are equal, to obtain mixed powder I;
[0136] The molar ratio of titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, tantalum carbide and hafnium carbide described in step 1② is 2:2:3:3:5:5;
[0137] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, tantalum carbide and hafnium carbide powders in step 1 is > 99.0wt.%;
[0138] 2. Mixing:
[0139] The metal carbide powder weighed in step 1① is preliminarily mixed with the mixed powder I weighed in step 1②, and then high-energy ball milling is performed in a vacuum environment to make the powders fully and evenly mixed, and the powders are crushed to reduce the particle size of the powders to improve their solid solution and sintering activity, thereby obtaining mixed powder II;
[0140] The process parameters of the high-energy ball milling in step 2 are: the ball-to-material ratio is 35:1, the speed of the ball mill is 350 r / min, the ball milling time is 10 h, and the materials of the ball mill and the grinding balls are both cemented carbide;
[0141] 3. Sintering:
[0142] The mixed powder II obtained in step 2 is placed in a mold and hot-pressed and sintered under vacuum to obtain a powder with the chemical formula (TiZrHfTa)C 0.8 Non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0143] The hot pressing sintering process described in step three is: heating from room temperature to 2000°C, keeping at 2000°C for 30 minutes, and then cooling to room temperature, with a heating rate of 30°C / min and a cooling rate of 10°C / min. The pressure is maintained at 50MPa during the sintering process.
[0144] Example 7 The chemical formula of the prepared product is (TiZrHfTa)C 0.8The non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content have uniform distribution of metal elements, a density of 98.9%, a hardness of 30.6GPa, a three-point bending strength of 461MPa, an elastic modulus of 433GPa, and a fracture toughness of 3.71MPa·m 1 / 2 .
[0145] Embodiment 8: A method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content is specifically completed by the following steps:
[0146] 1. The designed chemical formula is (TiZrHfNb)C 0.8 Non-stoichiometric multi-component carbide solid solution ceramics, weigh the required powder:
[0147] ①, weighing niobium carbide and hafnium carbide in equal molar ratio to obtain metal carbide powder;
[0148] ②, weigh titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, and the molar numbers of titanium carbide and zirconium carbide powders are equal, to obtain mixed powder I;
[0149] The molar ratio of titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and hafnium carbide described in step 1② is 2:2:3:3:5:5;
[0150] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide, niobium carbide and hafnium carbide powders in step 1 is > 99.0wt.%;
[0151] 2. Mixing:
[0152] The metal carbide powder weighed in step 1① is preliminarily mixed with the mixed powder I weighed in step 1②, and then high-energy ball milling is performed in a vacuum environment to make the powders fully and evenly mixed, and the powders are crushed to reduce the particle size of the powders to improve their solid solution and sintering activity, thereby obtaining mixed powder II;
[0153] The process parameters of the high-energy ball milling in step 2 are: the ball-to-material ratio is 35:1, the speed of the ball mill is 350 r / min, the ball milling time is 10 h, and the materials of the ball mill and the grinding balls are both cemented carbide;
[0154] 3. Sintering:
[0155] The mixed powder II obtained in step 2 is placed in a mold and hot-pressed and sintered under vacuum to obtain a powder with the chemical formula (TiZrHfNb)C 0.8 Non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content;
[0156] The hot pressing sintering process described in step three is: heating from room temperature to 1900°C, keeping at 1900°C for 10 minutes, and then cooling to room temperature, with a heating rate of 20°C / min and a cooling rate of 40°C / min. The pressure is maintained at 75MPa during the sintering process.
[0157] Example 8 The chemical formula of the prepared product is (TiZrHfNb)C 0.8 The non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content have uniform distribution of metal elements, a density of 99.7%, a hardness of 33.4GPa, a three-point bending strength of 438MPa, an elastic modulus of 459GPa, and a fracture toughness of 4.49MPa·m 1 / 2 .
[0158] Comparative Example 1: A method for preparing a non-stoichiometric multi-component carbide solid solution ceramic is specifically completed by the following steps:
[0159] 1. The designed chemical formula is (TiZrNb)C 0.9 Non-stoichiometric multi-component carbide solid solution ceramics, weigh the required powder:
[0160] ①. Weigh niobium carbide to obtain metal carbide powder;
[0161] ②, weigh titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, and the molar numbers of titanium carbide and zirconium carbide powders are equal, to obtain mixed powder I;
[0162] The molar ratio of titanium hydride, zirconium hydride, titanium carbide, zirconium carbide and niobium carbide described in step 1② is 3:3:17:17:20;
[0163] The purity of the titanium hydride, zirconium hydride, titanium carbide, zirconium carbide and niobium carbide powders in step 1 is > 99.0wt.%;
[0164] 2. Mixing:
[0165] The metal carbide powder weighed in step 1① is preliminarily mixed with the mixed powder I weighed in step 1②, and then high-energy ball milling is performed in a vacuum environment to make the powders fully and evenly mixed, and the powders are crushed to reduce the particle size of the powders to improve their solid solution and sintering activity, thereby obtaining mixed powder II;
[0166] The process parameters of the high-energy ball milling in step 2 are: a ball-to-material ratio of 50:1, a ball mill speed of 500 r / min, a ball milling time of 40 h, and the materials of the ball milling jar and the grinding balls are both cemented carbide;
[0167] 3. Sintering:
[0168] The mixed powder II obtained in step 2 is placed in a mold and spark plasma sintered under vacuum conditions to obtain a (TiZrNb)C 0.9 Non-stoichiometric multi-component carbide solid solution ceramics;
[0169] The spark plasma sintering process described in step three is: heating from room temperature to 1600°C, keeping at 1600°C for 30 minutes, and then cooling to room temperature, with a heating rate of 150°C / min and a cooling rate of 50°C / min. The pressure is maintained at 100MPa during the sintering process.
[0170] The chemical formula of the prepared sample 1 is (TiZrNb)C 0.9 The non-stoichiometric multi-component carbide solid solution ceramics were characterized and it was found that some metal elements were unevenly distributed. The density was only 95.8%, the hardness was 27.8GPa, the three-point bending strength was 324MPa, and the fracture toughness was 3.41MPa·m 1 / 2 By comparison, it can be found that the non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content prepared by the technical solution of the present invention have significant advantages in density and mechanical properties.
[0171] Comparative Example 2: A method for preparing a non-stoichiometric multi-component carbide solid solution ceramic is specifically completed by the following steps:
[0172] 1. The designed chemical formula is (TiZrNb)C 0.9 Non-stoichiometric multi-component carbide solid solution ceramics, weigh the required powder:
[0173] Weigh titanium metal, zirconium metal, niobium metal and graphite powder according to a molar ratio of 10:10:10:27; the purity of the titanium metal, zirconium metal, niobium metal and graphite powder in step 1 is > 98.0wt.%;
[0174] 2. Mixing:
[0175] The metal powder and graphite powder weighed in step 1 are preliminarily mixed, and then high-energy ball milling is performed in a vacuum environment to make the powders fully and evenly mixed, and the powders are crushed to reduce the particle size of the powders to improve their solid solution and sintering activity, thereby obtaining a mixed powder;
[0176] The process parameters of the high-energy ball milling in step 2 are: a ball-to-material ratio of 50:1, a ball mill speed of 500 r / min, a ball milling time of 40 h, and the materials of the ball milling jar and the grinding balls are both cemented carbide;
[0177] 3. Sintering:
[0178] The mixed powder obtained in step 2 is placed in a mold and spark plasma sintered under vacuum conditions to obtain a (TiZrNb)C 0.9 Non-stoichiometric multi-component carbide solid solution ceramics;
[0179] The spark plasma sintering process described in step three is: heating from room temperature to 2400°C, keeping at 2400°C for 30 minutes, and then cooling to room temperature, with a heating rate of 150°C / min and a cooling rate of 50°C / min. The pressure is maintained at 100MPa during the sintering process.
[0180] The chemical formula of the prepared sample 2 is (TiZrNb)C 0.9 The non-stoichiometric multi-component carbide solid solution ceramics were characterized and some oxide impurities were found. The density was 98.8%, the hardness was 29.1GPa, the three-point bending strength was 351MPa, and the fracture toughness was 3.38MPa·m 1 / 2 By comparison, it can be found that the non-stoichiometric multi-component carbide solid solution ceramics with high carbon vacancy content prepared by the technical solution of the present invention have significant advantages in density, mechanical properties and prevention of oxygen impurity introduction.
Claims
1. A method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content, characterized in that The preparation method is specifically completed according to the following steps:
1. Weigh the required powder: ①, weighing one of niobium carbide, tantalum carbide and hafnium carbide powders or weighing two or three of niobium carbide, tantalum carbide and hafnium carbide powders in equal molar ratio to obtain metal carbide powder; ②, weigh titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders, wherein the molar numbers of titanium hydride and zirconium hydride powders are equal, and the molar numbers of titanium carbide and zirconium carbide powders are equal, to obtain mixed powder I; The molar ratio of titanium hydride and titanium carbide described in Step 1② to the metal carbide powder weighed in Step 1① is , where 0.5 < x < 1.0, n is the sum of the types of metal carbides weighed in Step 1① and Step 1②, 3 ≤ n ≤ 5, and n is an integer; 2. Mixing: Preliminarily mixing the metal carbide powder weighed in step 1① with the mixed powder I weighed in step 1②, and then high-energy ball milling in an argon atmosphere or a vacuum environment to fully and evenly mix the powders, and crush the powders to reduce the particle size of the powders to improve their solid solution and sintering activity, to obtain mixed powder II; 3. Sintering: The mixed powder II obtained in step 2 is placed in a mold for sintering to obtain a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content.
2. The method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content according to claim 1, characterized in that The purity of the niobium carbide, tantalum carbide and hafnium carbide powders described in step 1① is all >99.0wt.%.
3. The method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content according to claim 1, characterized in that The purity of the titanium carbide, zirconium carbide, titanium hydride and zirconium hydride powders described in step 1② is all >99.0wt.%.
4. The method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content according to claim 1, characterized in that The ball-to-material ratio of the high-energy ball mill described in step 2 is (10-50):1, the rotation speed of the high-energy ball mill is 100 r / min-700 r / min, the time of the high-energy ball mill is 5 h-40 h, and the material of the ball mill jar and the grinding balls are both cemented carbide.
5. The method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content according to claim 1, characterized in that The sintering method described in step three is spark plasma sintering.
6. The method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content according to claim 5, characterized in that The spark plasma sintering process described in step three is: heating from room temperature to 1800~2400℃, keeping at 1800~2400℃ for 1min~30min, and then cooling to room temperature. The heating rate is 10℃ / min~200℃ / min, the cooling rate is 50℃ / min~200℃ / min, and the pressure is maintained at 10~100MPa during the sintering process.
7. The method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content according to claim 1, characterized in that The sintering method described in step three is hot pressing sintering.
8. The method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content according to claim 7, characterized in that The hot pressing sintering process described in step three is: heating from room temperature to 1800~2400℃, keeping at 1800~2400℃ for 1min~120min, and then cooling to room temperature, with a heating rate of 5℃ / min~30℃ / min, a cooling rate of 5℃ / min~50℃ / min, and maintaining a pressure of 10MPa~100MPa during the sintering process.
9. The method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content according to claim 1, characterized in that During the sintering process in step 3, an inert gas needs to be continuously introduced to form a protective atmosphere or maintain a vacuum state; the inert gas is argon, helium or krypton; and the vacuum state is <20Pa.
10. The method for preparing a non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content according to claim 1, characterized in that The chemical formula of the non-stoichiometric multi-component carbide solid solution ceramic with a high carbon vacancy content described in step three is (TiZrM)C x , (TiZrM1M2)C x , (TiZrM1M2M3)C x , where 0.5 < x < 1.0, M is one of Nb, Ta, and Hf; M1M2 are two of Nb, Ta, and Hf; M1M2M3 are Nb, Ta, and Hf.
Citation Information
Patent Citations
Preparation technology of transition metal carbide powder and transition metal carbide-nitride compound powder
CN108975339A
Method for preparing MAX-phase high-entropy ceramic material
CN113185295A
Method for preparing titanium subgroup carbonitride solid solution composite ceramic material by sintering
CN113929463A
Non-stoichiometric-ratio carbide-doped tungsten-based hot cathode material and preparation method thereof
CN117363944A
Composite material and method for preparing the same
US20180334410A1