A method for preparing 1,4-butanediamine by Raney nickel catalytic hydrogenation

Core-shell catalysts are prepared by Rainey nickel catalyst and support, and 1,4-butanediamine is prepared by low-pressure hydrogenation reaction, which solves the problems of high production costs and expensive catalysts in the prior art, and achieves high efficiency and economical butanediamine Production.

CN118005517BActive Publication Date: 2024-12-06HE NAN NENG YUAN JI TUAN YAN JIU ZONG YUAN YOU XIAN GONG SI +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410157117.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-04
Publication Date
2024-12-06
Estimated Expiration
2044-02-04

AI Technical Summary

Technical Problem

In the prior art, the production cost of butadiene is high, the catalyst is expensive, and the chemical synthesis method relies on expensive alkaline catalysts and high-energy-consuming fluidized bed reactors, which is difficult to meet market demand.

Method used

The core-shell catalyst Ni@C was prepared using Rainey nickel catalyst and support (such as polydopamine or glucose), and 1,4-butanediamine was prepared by hydrogenation reaction under low pressure and mild conditions, using water, ethanol and tetrahydrofuran. The solvent reacts.

Benefits of technology

It has achieved efficient preparation of butadiene, good catalyst selectivity and stability, reduced by-products, improved main product selectivity, simple and cost-effective process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118005517B_ABST
    Figure CN118005517B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing 1,4-diamine by catalytic hydrogenation of Raney nickel, belongs to the technical field of diamine synthesis, and uses a carrier added to Raney nickel to obtain a core-shell catalyst Ni@C; subsequently, 1,4-dimethylformonitrile, a solvent and a core-shell catalyst are added to a reactor and hydrogen is passed through after mixing, and a hydrogenation reaction is performed to obtain 1,4-diamine. 1,4-diamine is prepared using the method of the present invention, and the reaction conditions are simple, the reaction unit is less, and the by-product is pyrrolidine and polymer, and the selectivity of the main product 1,4-diamine is greatly improved. Therefore, the technology has great economic value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of butanediamine synthesis, in particular to a method for preparing 1,4-butanediamine by Raney nickel catalytic hydrogenation. Background Art

[0002] Butanediamine includes 1,2-butanediamine, 1,3-butanediamine, 2,3-butanediamine and 1,4-butanediamine. Among them, 1,4-butanediamine is also called putrescine. In cells, 1,4-butanediamine is produced by ornithine under the action of ornithine decarboxylase. 1,4-Butanediamine can be used as a chemical intermediate, a raw material for the new polyamide variety nylon 46, and in pharmaceutical and biochemical research. It has important industrial uses. With the development of society, the application scope of butanediamine is constantly expanding and the market demand is growing. However, domestic manufacturers have not carried out large-scale production, and domestic products are relatively few. They mainly rely on imports and are expensive.

[0003] At present, the methods for synthesizing butanediamine include chemical synthesis and biosynthesis. Generally, the enzymes suitable for these processes in the biosynthesis of butanediamine are expensive, and it is also laborious and expensive to separate butanediamine from highly diluted fermentation broth, and the cost of raw materials is high. Therefore, the synthesis of butanediamine is mainly based on chemical synthesis.

[0004] The chemical synthesis method is the main method for producing butanediamine. Butanediamine is mainly produced by chemical synthesis of acrylonitrile: acrylonitrile and hydrocyanic acid are used as raw materials to synthesize succinonitrile under the action of alkaline catalyst, and succinonitrile is hydrogenated to obtain butanediamine.

[0005] In the prior art, there is a method for preparing diamines from aliphatic dinitriles using a modified supported Ni-Co-Pb catalyst, which uses a fluidized bed reactor and dialkoxymethane as a solvent for direct hydrogenation. This process method for preparing the target product has the advantages of low energy consumption, high dinitriles conversion rate and selectivity, high catalyst efficiency, green environmental protection, and easy industrial production. The disadvantage is that the catalyst is expensive.

[0006] Therefore, it is necessary to provide a method for preparing 1,4-butanediamine to solve the above problems. Summary of the invention

[0007] The invention aims to provide a method for preparing 1,4-butanediamine by catalytic hydrogenation of Raney nickel. The method of the invention has the advantages of simple reaction conditions, less reaction units and high product conversion rate for preparing 1,4-butanediamine.

[0008] To achieve the above object, the present invention provides a method for preparing 1,4-butanediamine by catalytic hydrogenation of Raney nickel, comprising the following steps:

[0009] S1. Preparation of core-shell catalyst: adding a carrier to Raney nickel to obtain a core-shell catalyst Ni@C;

[0010] S2, hydrogenation reaction: 1,4-succinonitrile, a solvent and a core-shell catalyst prepared by S1 are added into a reactor, and then hydrogen is introduced to carry out a hydrogenation reaction to obtain 1,4-butanediamine.

[0011] Preferably, the carrier in step S1 is any one of polydopamine and glucose.

[0012] Preferably, when the carrier in step S1 is polydopamine, the preparation of the core-shell catalyst comprises the following steps:

[0013] (1) Add polydopamine to the aqueous solution of Raney nickel and stir for 2 h;

[0014] (2) subjecting the product prepared in step (1) to rotary evaporation to remove water and obtain a wet product;

[0015] (3) The wet product was placed in an inert atmosphere and calcined at 800°C for 5 h to obtain a core-shell catalyst Ni@C.

[0016] Preferably, when the carrier in step S1 is glucose, the preparation of the core-shell catalyst comprises the following steps:

[0017] (1) Add glucose to the aqueous solution of Raney nickel and stir for 2 h;

[0018] (2) hydrothermally treating the product prepared in step (1) at 180° C. for 1 h to obtain a wet product;

[0019] (3) The wet product was placed in an inert atmosphere and calcined at 800°C for 5 h to obtain a core-shell catalyst Ni@C.

[0020] Preferably, the solvent in step S2 is a mixed solvent of water, ethanol, 1,4-dioxane and tetrahydrofuran.

[0021] Preferably, the temperature of the hydrogenation reaction in step S2 is 80° C., the reaction time is 1 h, and the pressure in the reaction system is 8 MPa.

[0022] Therefore, the present invention adopts the above-mentioned method of preparing 1,4-butanediamine by Raney nickel catalytic hydrogenation, which has the following beneficial effects:

[0023] The present invention uses 1,4-butanediamine as a raw material and obtains butanediamine through a hydrogenation reaction, providing a process route with a simple process and extremely high efficiency and yield. At the same time, the catalyst prepared by the above-mentioned preparation method has good selectivity and stability, and the catalytic activity and selectivity do not change after repeated use. The process is simple and the by-products are pyrrolidine and polymers, and the selectivity of the main product 1,4-butanediamine is greatly improved. Therefore, the technology has great economic value.

[0024] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0026] Figure 1 This is the SEM image of the core-shell catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0028] Unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The words "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. "Include" or "comprise" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connect" or "connected" and similar words are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0029] As shown in the figure, the present invention provides a method for preparing 1,4-butanediamine by Raney nickel catalytic hydrogenation, comprising the following steps:

[0030] S1. Preparation of core-shell catalyst: adding a carrier to Raney nickel to obtain a core-shell catalyst Ni@C;

[0031] S2, hydrogenation reaction: 1,4-succinonitrile, a solvent and a core-shell catalyst prepared by S1 are added into a reactor, and then hydrogen is introduced to carry out a hydrogenation reaction to obtain 1,4-butanediamine.

[0032] In step S1, the carrier is any one of polydopamine and glucose.

[0033] When the carrier in step S1 is polydopamine, the preparation of the core-shell catalyst comprises the following steps:

[0034] (1) Add polydopamine to the aqueous solution of Raney nickel and stir for 2 h;

[0035] (2) subjecting the product prepared in step (1) to rotary evaporation to remove water and obtain a wet product;

[0036] (3) The wet product was placed in an inert atmosphere and calcined at 800°C for 5 h to obtain a core-shell catalyst Ni@C.

[0037] When the carrier in step S1 is glucose, the preparation of the core-shell catalyst comprises the following steps:

[0038] (1) Add glucose to the aqueous solution of Raney nickel and stir for 2 h;

[0039] (2) hydrothermally treating the product prepared in step (1) at 180° C. for 1 h to obtain a wet product;

[0040] (3) The wet product was placed in an inert atmosphere and calcined at 800°C for 5 h to obtain a core-shell catalyst Ni@C.

[0041] The solvent in step S2 is a mixed solvent of water, ethanol, 1,4-dioxane and tetrahydrofuran.

[0042] The temperature of the hydrogenation reaction in step S2 is 80° C., the reaction time is 1 h, and the pressure in the reaction system is 8 MPa.

[0043] The technical solution of the present invention is further illustrated by the following examples.

[0044] Example 1

[0045] This embodiment provides a method for preparing 1,4-butanediamine by catalytic hydrogenation of Raney nickel, which is prepared by the following steps:

[0046] (1) Commercial Raney nickel was used, glucose was added to the aqueous solution of Raney nickel, and the mixture was hydrothermally heated at 180°C for 1 h to obtain a wet product. The wet product was calcined at 800°C for 5 h in an inert atmosphere to obtain a core-shell catalyst Ni@C.

[0047] (2) 1,4-butanedionitrile, water, ethanol, 1,4-dioxane, tetrahydrofuran and core-shell catalyst Ni@C were added into a reactor, and hydrogen was introduced after mixing. The temperature in the reactor was adjusted to 80° C. and the pressure was adjusted to 8 MPa. After reacting for 1 hour, a hydrogenation reaction was carried out to obtain 1,4-butanediamine.

[0048] The obtained 1,4-butanediamine product was sampled and tested, and the test results are shown in Table 1.

[0049] Example 2

[0050] This embodiment provides a method for preparing 1,4-butanediamine by catalytic hydrogenation of Raney nickel, which is prepared by the following steps:

[0051] (1) using commercial Raney nickel, adding polydopamine to the aqueous solution of Raney nickel, and stirring for 2 hours; performing rotary evaporation to remove water from the prepared product to obtain a wet product; and calcining the product at 800° C. in an inert atmosphere for 5 hours to obtain a core-shell catalyst Ni@C;

[0052] (2) 1,4-butanedionitrile, water, ethanol, 1,4-dioxane, tetrahydrofuran and core-shell catalyst Ni@C were added into a reactor, and hydrogen was introduced after mixing. The temperature in the reactor was adjusted to 80° C. and the pressure was adjusted to 8 MPa. After reacting for 1 hour, a hydrogenation reaction was carried out to obtain 1,4-butanediamine.

[0053] The obtained 1,4-butanediamine product was sampled and tested, and the test results are shown in Table 1.

[0054] Example 3

[0055] This embodiment provides a method for preparing 1,4-butanediamine by catalytic hydrogenation of Raney nickel, which is prepared by the following steps:

[0056] (1) using commercial Raney nickel, adding polydopamine to the aqueous solution of Raney nickel, stirring for 2 hours; performing rotary evaporation to remove water from the prepared product to obtain a wet product; placing the product in an inert atmosphere and calcining it at 850° C. for 5 hours to obtain a core-shell catalyst Ni@C;

[0057] (2) 1,4-butanedionitrile, water, ethanol, 1,4-dioxane, tetrahydrofuran and core-shell catalyst Ni@C were added into a reactor, and hydrogen was introduced after mixing. The temperature in the reactor was adjusted to 80° C. and the pressure was adjusted to 8 MPa. After reacting for 1 hour, a hydrogenation reaction was carried out to obtain 1,4-butanediamine.

[0058] The obtained 1,4-butanediamine product was sampled and tested, and the test results are shown in Table 1.

[0059] The degree of hydrogenation, conversion rate and selectivity of Examples 1-3 of the present invention are listed in Table 1.

[0060] Table 1 Hydrogenation degree, conversion rate and selectivity of Examples 1-2

[0061]

[0062] It can be seen from the above examples and Table 1 that the selective hydrogenation of 1,4-butanediamine catalyzed by Raney nickel using the catalyst provided by the present invention has a high degree of hydrogenation, a simple process, and by-products are pyrrolidine and oligomers, and the selectivity of the main product 1,4-butanediamine is greatly improved.

[0063] Therefore, the purpose of the present invention is to provide a method for preparing 1,4-butanediamine by Raney nickel catalytic hydrogenation. The method of the present invention is used to prepare 1,4-butanediamine, and the reaction conditions are simple, the reaction units are relatively few, and the by-products are pyrrolidine and polymers, and the selectivity of the main product 1,4-butanediamine is greatly improved. Therefore, the technology has great economic value.

[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing 1,4-butanediamine by Raney nickel catalytic hydrogenation, characterized in that: The following steps are involved: S1. Preparation of core-shell catalyst: adding a carrier to Raney nickel to obtain a core-shell catalyst Ni@C; S2, hydrogenation reaction: 1,4-succinonitrile, a solvent and a core-shell catalyst prepared by S1 are added into a reactor, and then hydrogen is introduced to carry out a hydrogenation reaction to obtain 1,4-butanediamine; Step S1: the carrier is any one of polydopamine and glucose; In step S2, the temperature of the hydrogenation reaction is 80°C, the reaction time is 1h, and the pressure in the reaction system is 8MPa; When the carrier in step S1 is polydopamine, the preparation of the core-shell catalyst comprises the following steps: (1) Add polydopamine to the aqueous solution of Raney nickel and stir for 2 h; (2) subjecting the product prepared in step (1) to rotary evaporation to remove water and obtain a wet product; (3) The wet product was placed in an inert atmosphere and calcined at 800-1000 °C for 5 h to obtain a core-shell catalyst Ni@C; Or when the carrier in step S1 is glucose, the preparation of the core-shell catalyst comprises the following steps: (1) Add glucose to the aqueous solution of Raney nickel and stir for 2 h; (2) hydroheating the product prepared in step (1) at 180° C. for 1 h to obtain a wet product; (3) The wet product was placed in an inert atmosphere and calcined at 800 °C for 5 h to obtain a core-shell catalyst Ni@C.

2. The method for preparing 1,4-butanediamine by Raney nickel catalytic hydrogenation according to claim 1, characterized in that: The solvent in step S2 is a mixed solvent of water, ethanol, 1,4-dioxane and tetrahydrofuran.