Double-lapped double polymer membrane-based waterproofing coiled material with good flexibility and preparation method thereof
By introducing modified calcium carbonate and silica into the waterproof membrane, adjusting their mass ratio, and using a superimposed hot-pressing composite process, the problems of low flexibility and peel strength of the waterproof membrane are solved, and the waterproof performance of the membrane is significantly improved. and service life.
Patent Information
- Application Number
- CN202410165252.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-02-05
AI Technical Summary
Existing waterproof membranes are weak in flexibility and easily damaged, and the peel strength at the overlap is low, which affects the waterproofing effect and service life.
It adopts a double-overlapping double-polymer film-based waterproofing membrane structure, including an anti-adhesive protective layer, a multi-layer adhesive layer and a polymer layer. By adding modified calcium carbonate and white carbon black to the polymer layer, the mass ratio is adjusted. , improve tensile strength and peel strength, and are prepared through a superimposed hot pressing composite process.
It significantly improves the maximum tensile force of the waterproof membrane, the elongation at the maximum tensile force and the peel strength between polymer layers, enhances the flexibility of the membrane and the strength of the overlap, and extends the service life.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of waterproof coiled materials, and in particular to a double-lapped double-polymer membrane-based waterproof coiled material with good flexibility and a preparation method thereof. Background Art
[0002] Waterproofing membrane is the most widely used waterproofing material in construction projects, and plays a vital role in ensuring the quality of the project. Waterproofing membranes cannot be continuous and need to be connected by seams to achieve a waterproof effect.
[0003] However, the structure of waterproof membranes is diverse and the construction process is complicated. In actual applications, there are often problems such as insufficient overlap of the membranes, cracking and leakage at the overlapped parts of the membranes. In addition, the existing waterproof membranes are less flexible and are easily damaged by sharp objects. Therefore, the overlap quality and the flexibility of the waterproof membranes are important factors affecting the waterproof effect of the membranes. Therefore, it is necessary to improve the flexibility of the waterproof membranes and the peeling strength of the overlapped parts so that the waterproof membranes have a longer service life. Summary of the invention
[0004] The invention provides a double-lapped double-polymer membrane-based waterproofing coiled material with good flexibility and a preparation method thereof, which solves the problems of low peeling strength and low flexibility at the overlapping parts of the waterproofing coiled material in the related art.
[0005] The technical solution of the present invention is as follows:
[0006] The present invention provides a double-lapped double polymer membrane-based waterproofing coiled material with good flexibility, wherein the waterproofing coiled material comprises, from top to bottom, an anti-adhesive protective layer, a first adhesive layer, a first polymer layer, a second adhesive layer, a second polymer layer, a third adhesive layer, and an isolation film layer;
[0007] The first adhesive layer, the second adhesive layer and the third adhesive layer each independently comprise the following raw materials in parts by weight: 40-50 parts of butyl rubber, 10-15 parts of tackifying resin, 8-12 parts of white carbon black, 1-1.5 parts of vulcanizing agent I, 1-2 parts of antioxidant I, and 0.5-1 parts of coupling agent;
[0008] The first polymer layer and the second polymer layer each independently include the following raw materials in parts by weight: 40 to 45 parts of EPDM rubber, 12 to 16 parts of modified calcium carbonate, 1 to 2 parts of paraffin wax, 0.5 to 1 part of zinc oxide, 3 to 6 parts of stearic acid, 2 to 5 parts of accelerator M, 1 to 2 parts of antioxidant II, and 1 to 1.5 parts of vulcanizer II. The modified calcium carbonate is calcium carbonate modified by 4,4'-diaminostilbene-2,2'-disulfonic acid.
[0009] As a further technical solution, the vulcanizing agent I and the vulcanizing agent II each independently include one or two of sulfur and dicumyl peroxide.
[0010] As a further technical solution, the antioxidant I and the antioxidant II each independently include one or two of the antioxidant OD and the antioxidant MB.
[0011] As a further technical solution, the coupling agent is a silane coupling agent.
[0012] As a further technical solution, the preparation method of the modified calcium carbonate is to add 4,4'-diaminostilbene-2,2'-disulfonic acid into an ethanol solution and mix evenly, and then add calcium carbonate for modification to obtain modified calcium carbonate.
[0013] As a further technical solution, the modification temperature is 50-60°C, and the modification time is 1-2h.
[0014] As a further technical solution, the added amount of 4,4'-diaminostilbene-2,2'-disulfonic acid is 3-5% of the mass of calcium carbonate.
[0015] As a further technical solution, the mass ratio of the modified calcium carbonate to white carbon black is 1~2:1.
[0016] As a further technical solution, the mass ratio of the modified calcium carbonate to white carbon black is 1.5:1.
[0017] The present invention finds that by limiting the mass ratio of modified calcium carbonate and white carbon black, the tensile strength and elongation at break of the polymer layer and the peeling strength between the polymer layers can be improved.
[0018] As a further technical solution, the first adhesive layer, the second adhesive layer and the third adhesive layer are independently obtained by uniformly mixing the raw materials, kneading and extruding.
[0019] As a further technical solution, the first polymer layer and the second polymer layer are prepared independently by uniformly mixing the raw materials, followed by kneading and extrusion.
[0020] As a further technical solution, the thickness of the first adhesive layer, the second adhesive layer and the third adhesive layer are each independently 0.3-1.0 mm.
[0021] As a further technical solution, the thickness of the first polymer layer and the second polymer layer are independently 0.1-1.0 mm.
[0022] The present invention also includes a method for preparing a double-lap double-polymer membrane-based waterproof roll with good flexibility, comprising the following steps: in order from top to bottom: anti-sticking protective layer, first adhesive layer, first polymer layer, second adhesive layer, second polymer layer, third adhesive layer, isolation film layer, superimposing and hot-pressing to obtain a double-lap double-polymer membrane-based waterproof roll.
[0023] As a further technical solution, the isolation film layer is a polyethylene isolation film.
[0024] As a further technical solution, the anti-sticking protective layer is an anti-sticking silicone oil isolation film.
[0025] The working principle and beneficial effects of the present invention are:
[0026] 1. The present invention is a double-lapped double polymer membrane-based waterproofing coiled material, in which calcium carbonate modified by 4,4'-diaminostilbene-2,2'-disulfonic acid is added to the polymer layer. The addition of modified calcium carbonate not only improves the maximum tensile force and elongation at maximum tensile force of the waterproofing coiled material, but also further improves the peel strength between the first polymer layer and the second polymer layer in the high waterproofing coiled material. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] In the following embodiments and comparative examples:
[0029] Butyl rubber: Exxon 268S;
[0030] Tackifying resin: phenolic resin White Shark 2402;
[0031] EPDM rubber: Shanghai Sinopec Mitsui 3092PM;
[0032] White carbon black: particle size 2000 mesh, content 99%;
[0033] Calcium carbonate: particle size 1250 mesh;
[0034] The isolation film layer is a polyethylene isolation film;
[0035] The anti-sticking protective layer is an anti-sticking silicone oil isolation film.
[0036] Example 1
[0037] A method for preparing a double-lapped double polymer membrane-based waterproofing coiled material with good flexibility comprises the following steps:
[0038] S1. 40 parts of butyl rubber, 10 parts of tackifying resin, 10 parts of white carbon black, 1 part of antioxidant OD, and 0.5 parts of silane coupling agent KH-550 were mixed evenly and put into an internal mixer and kneaded at 130° C. for 20 minutes, and then 1 part of sulfur was added and kneaded for 15 minutes. The mixture was extruded, and the first adhesive layer, the second adhesive layer, and the third adhesive layer were obtained by pulling, calendering, and cooling, each having a thickness of 0.5 mm;
[0039] S2, 40 parts of EPDM rubber, 12 parts of modified calcium carbonate, 1 part of polyethylene glycol, 2 parts of accelerator M, and 1 part of antioxidant OD were mixed evenly, added to an internal mixer, kneaded at 135°C for 8 minutes, filtered, 0.5 parts of zinc oxide and 3 parts of stearic acid were added to mix at 100°C, rested for 24 hours, 1 part of sulfur was added to vulcanize at 180°C, and then extruded, and the first polymer layer and the second polymer layer with a thickness of 0.7 mm were obtained after traction, calendering, and cooling; wherein the vulcanization speed was 7m / min;
[0040] S3, in the order of anti-adhesion protective layer, first adhesive layer, first polymer layer, second adhesive layer, second polymer layer, third adhesive layer, and isolation film from top to bottom, after superposition and hot pressing, a double-lapped double polymer membrane-based waterproofing membrane is obtained;
[0041] The preparation method of the modified calcium carbonate is as follows: 0.9 g of 4,4'-diaminostilbene-2,2'-disulfonic acid is added to 300 mL of ethanol aqueous solution (the volume ratio of anhydrous ethanol to water is 95:5) and mixed evenly, and then 30 g of calcium carbonate is added and modified at 50° C. for 2 hours to obtain modified calcium carbonate.
[0042] Example 2
[0043] A method for preparing a double-lapped double polymer membrane-based waterproofing coiled material with good flexibility comprises the following steps:
[0044] S1. 45 parts of butyl rubber, 12 parts of tackifying resin, 12 parts of white carbon black, 1.5 parts of antioxidant OD, and 0.8 parts of silane coupling agent KH-550 were mixed evenly and put into an internal mixer and kneaded at 130° C. for 20 minutes, and then 1.2 parts of sulfur were added and kneaded for 15 minutes. The mixture was extruded, and the first adhesive layer, the second adhesive layer, and the third adhesive layer were obtained by traction, calendaring, and cooling, each having a thickness of 0.3 mm;
[0045] S2. After uniformly mixing 42 parts of EPDM rubber, 12 parts of modified calcium carbonate, 1.5 parts of paraffin wax, 4 parts of accelerator M and 1.5 parts of antioxidant OD, the mixture was added into an internal mixer and mixed at 135°C for 8 minutes, filtered, 0.5-1 parts of zinc oxide and 5 parts of stearic acid were added to mix the rubber at 100°C, left to rest for 24 hours, 1.2 parts of sulfur were added to vulcanize at 180°C and then extruded, and the first and second polymer layers were obtained with a thickness of 0.1 mm after traction, calendering and cooling; wherein the vulcanization speed was 7 m / min;
[0046] S3, in the order of anti-adhesion protective layer, first adhesive layer, first polymer layer, second adhesive layer, second polymer layer, third adhesive layer, and isolation film from top to bottom, after superposition and hot pressing, a double-lapped double polymer membrane-based waterproofing membrane is obtained;
[0047] The preparation method of the modified calcium carbonate is as follows: 0.9 g of 4,4'-diaminostilbene-2,2'-disulfonic acid is added to 300 mL of ethanol aqueous solution (the volume ratio of anhydrous ethanol to water is 95:5) and mixed evenly, and then 30 g of calcium carbonate is added and modified at 55° C. for 1.5 h to obtain modified calcium carbonate.
[0048] Example 3
[0049] A method for preparing a double-lapped double polymer membrane-based waterproofing coiled material with good flexibility comprises the following steps:
[0050] S1. 50 parts of butyl rubber, 15 parts of tackifying resin, 8 parts of white carbon black, 2 parts of antioxidant MB and 1 part of silane coupling agent KH-550 were mixed evenly and put into an internal mixer and kneaded at 130° C. for 20 minutes, and then 1.5 parts of sulfur were added and kneaded for 15 minutes. The mixture was extruded, and the first, second and third adhesive layers with a thickness of 1.0 mm were obtained by traction, calendering and cooling.
[0051] S2. After uniformly mixing 45 parts of EPDM rubber, 14 parts of modified calcium carbonate, 2 parts of paraffin wax, 5 parts of accelerator M and 2 parts of antioxidant MB, the mixture was added into an internal mixer and mixed at 135°C for 8 minutes, filtered, 1 part of zinc oxide and 3-6 parts of stearic acid were added to mix the rubber at 100°C, left to rest for 24 hours, 1.5 parts of sulfur were added to vulcanize at 180°C and then extruded, and the first and second polymer layers with a thickness of 1.0 mm were obtained after traction, calendering and cooling; wherein the vulcanization speed was 7 m / min;
[0052] S3, in the order of anti-adhesion protective layer, first adhesive layer, first polymer layer, second adhesive layer, second polymer layer, third adhesive layer, and isolation film from top to bottom, after superposition and hot pressing, a double-lapped double polymer membrane-based waterproofing membrane is obtained;
[0053] The preparation method of the modified calcium carbonate is as follows: 0.9 g of 4,4'-diaminostilbene-2,2'-disulfonic acid is added to 300 mL of ethanol aqueous solution (the volume ratio of anhydrous ethanol to water is 95:5) and mixed evenly, and then 30 g of calcium carbonate is added and modified at 60° C. for 1 hour to obtain modified calcium carbonate.
[0054] Example 4
[0055] The only difference between this embodiment and embodiment 1 is that the amount of 4,4'-diaminostilbene-2,2'-disulfonic acid is 1.2 g.
[0056] Example 5
[0057] The only difference between this embodiment and embodiment 1 is that the amount of 4,4'-diaminostilbene-2,2'-disulfonic acid is 1.5 g.
[0058] Example 6
[0059] The only difference between this comparative example and Example 2 is that the modified calcium carbonate is 14.4 parts and the white carbon black is 9.6 parts.
[0060] Example 7
[0061] The only difference between this comparative example and Example 2 is that the amount of modified calcium carbonate is 16 parts and the amount of white carbon black is 8 parts.
[0062] Comparative Example 1
[0063] A method for preparing a double-lapped double polymer membrane-based waterproofing coiled material with good flexibility comprises the following steps:
[0064] S1. 40 parts of butyl rubber, 10 parts of tackifying resin, 10 parts of white carbon black, 1 part of antioxidant OD, and 0.5 parts of silane coupling agent KH-550 were mixed evenly and put into an internal mixer and mixed at 130° C. for 20 minutes, and then 1 part of sulfur was added and mixed for 15 minutes. The mixture was extruded, and the first adhesive layer, the second adhesive layer, and the third adhesive layer were obtained by pulling, calendering, and cooling, each having a thickness of 0.3 mm;
[0065] S2. Evenly mix 40 parts of EPDM rubber, 12 parts of calcium carbonate, 1 part of polyethylene glycol, 2 parts of accelerator M and 1 part of antioxidant OD, add into internal mixer and mix at 135°C for 8 minutes, filter, add 0.5 parts of zinc oxide and 3 parts of stearic acid and mix at 100°C, let it rest for 24 hours, add 1 part of sulfur and vulcanize at 180°C, then extrude, and obtain the first polymer layer and the second polymer layer with a thickness of 0.1 mm after traction, calendering and cooling; wherein the vulcanization speed is 7 m / min.
[0066] S3. The order from top to bottom is: anti-sticking protective layer, first adhesive layer, first polymer layer, second adhesive layer, second polymer layer, third adhesive layer, and isolation film. After superposition and hot pressing, a double-lapped double polymer membrane-based waterproofing membrane is obtained.
[0067] Comparative Example 2
[0068] The difference between this comparative example and Example 1 lies in the modified calcium carbonate. The preparation method of the modified calcium carbonate in this comparative example is as follows: 0.9 g of γ-methacryloxypropyltrimethoxysilane is added to 300 mL of ethanol aqueous solution (the volume ratio of anhydrous ethanol to water is 95:5) and mixed evenly, and then 30 g of calcium carbonate is added and modified at 50° C. for 2 h to obtain modified calcium carbonate.
[0069] Test example
[0070] According to the measurement method in GB / 35467-2017 "Wet-laid waterproof membrane", the maximum tensile force (transverse), the elongation at maximum tensile force (transverse) and the peel strength between the first polymer layer and the second polymer layer of the waterproof membrane in Examples 1 to 7 and Comparative Examples 1 to 2 were measured. The measurement results are shown in Table 1.
[0071] Table 1 Performance test results of waterproof membranes in Examples 1 to 7 and Comparative Examples 1 to 2
[0072]
[0073] Compared with Example 1, the calcium carbonate in Example 1 is not modified, and the calcium carbonate in Example 2 is modified using γ-methacryloxypropyltrimethoxysilane. As a result, the maximum tensile force and elongation at maximum tensile force of the waterproof membrane in Examples 1~2 are lower than those in Example 1, and the peel strength between the first polymer layer and the second polymer is also lower than that in Example 1, indicating that the use of 4,4'-diaminobis(phenylethylene)-2,2'-disulfonic acid to modify calcium carbonate can improve the maximum tensile force and elongation at maximum tensile force of the waterproof membrane and the peel strength between the first polymer layer and the second polymer.
[0074] Compared with Example 2, Examples 6~7 change the mass ratio of modified calcium carbonate and white carbon black. As a result, the maximum tensile force and elongation at maximum tensile force of the waterproof membrane in Example 6 are higher than those in Example 2 and Example 7, and the peel strength between the first polymer layer and the second polymer is also higher than that in Example 2 and Example 7, indicating that when the mass ratio of modified calcium carbonate and white carbon black is 1.5:1, not only the maximum tensile force and elongation at maximum tensile force of the waterproof membrane can be further improved, but also the peel strength between the first polymer layer and the second polymer can be further improved.
[0075] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A double-lapped double polymer membrane-based waterproofing coiled material with good flexibility, wherein the waterproofing coiled material comprises, from top to bottom, an anti-adhesive protective layer, a first adhesive layer, a first polymer layer, a second adhesive layer, a second polymer layer, a third adhesive layer, and an isolation film layer; It is characterized in that The first adhesive layer, the second adhesive layer and the third adhesive layer each independently comprise the following raw materials in parts by weight: 40-50 parts of butyl rubber, 10-15 parts of tackifying resin, 8-12 parts of white carbon black, 1-1.5 parts of vulcanizing agent I, 1-2 parts of antioxidant I, and 0.5-1 parts of coupling agent; The first polymer layer and the second polymer layer each independently include the following raw materials in parts by weight: 40 to 45 parts of EPDM rubber, 12 to 16 parts of modified calcium carbonate, 1 to 2 parts of paraffin wax, 0.5 to 1 part of zinc oxide, 3 to 6 parts of stearic acid, 2 to 5 parts of accelerator M, 1 to 2 parts of antioxidant II, and 1 to 1.5 parts of vulcanizer II; the modified calcium carbonate is calcium carbonate modified by 4,4'-diaminostilbene-2,2'-disulfonic acid.
2. A flexible double-lapped double polymer membrane-based waterproofing coiled material according to claim 1, characterized in that: The coupling agent is a silane coupling agent.
3. The double-lapped double polymer membrane-based waterproofing coiled material with good flexibility according to claim 1, characterized in that: The preparation method of the modified calcium carbonate comprises the following steps: adding 4,4'-diaminostilbene-2,2'-disulfonic acid into an ethanol solution and mixing the mixture evenly; and then adding calcium carbonate for modification to obtain the modified calcium carbonate.
4. The double-lapped double polymer membrane-based waterproofing coiled material with good flexibility according to claim 1, characterized in that: The modification temperature is 50-60° C., and the modification time is 1-2 hours.
5. The double-lapped double polymer membrane-based waterproofing coiled material with good flexibility according to claim 1, characterized in that: The added amount of the 4,4'-diaminostilbene-2,2'-disulfonic acid is 3-5% of the mass of calcium carbonate.
6. The double-lapped double polymer membrane-based waterproofing coiled material with good flexibility according to claim 1, characterized in that: The mass ratio of the modified calcium carbonate to white carbon black is 1-2:
1.
7. The double-lapped double polymer membrane-based waterproofing coiled material with good flexibility according to claim 1, characterized in that: The first polymer layer and the second polymer layer are prepared independently by uniformly mixing the raw materials, followed by kneading and extruding.
8. The flexible double-lapped double polymer membrane-based waterproofing coiled material according to claim 1, characterized in that: The thickness of the first adhesive layer, the second adhesive layer and the third adhesive layer are each independently 0.3-1.0 mm.
9. The double-lapped double polymer membrane-based waterproofing coiled material with good flexibility according to claim 1, characterized in that: The thickness of the first polymer layer and the second polymer layer are each independently 0.1 to 1.0 mm.
10. A method for preparing a flexible double-lapped double polymer membrane-based waterproofing coiled material according to any one of claims 1 to 9, characterized in that: The following steps are involved: The order from top to bottom is: anti-sticking protective layer, first adhesive layer, first polymer layer, second adhesive layer, second polymer layer, third adhesive layer, isolation film layer. After superposition and hot pressing, a double-lapped double polymer membrane-based waterproofing membrane is obtained.