A method for preparing a 3D printed porous bioceramic artificial eye base
Preparing porous bioceramic prosthetic eye sockets through 3D printing technology solves the problems of insufficient biocompatibility and high production cost of existing prosthetic eye socket materials, and realizes an aluminum oxide prosthetic eye socket with low density, wear resistance and high stability. Reduced implant exposure and improved biocompatibility and integration.
Patent Information
- Application Number
- CN202410260506.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-07
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-03-07
AI Technical Summary
Existing prosthetic eye platform materials have problems such as insufficient biocompatibility, high production costs, and high post-implantation exposure rate. In particular, hydroxyapatite and high-density polyethylene materials have poor performance in seed cell attachment and growth, and are prone to oxidation. Although aluminum materials have good biocompatibility, they have high density, which affects the integration of implants.
Porous bioceramic prosthetic eye sockets are prepared using 3D printing technology. By preparing alumina and pseudo-boehmite powder, combined with PVA binder and supporting materials, SOLIDWORKS is used to design the model and printed through 3D-Bioplotter to control the pore structure and pore size. , to improve fibrous tissue attachment and growth and reduce implant exposure rate.
A low-density, wear-resistant, and highly stable alumina bioceramic prosthetic eye platform has been realized, which reduces the exposure rate of the implant, lowers the production cost, promotes the growth of fibrous tissue, and improves the biocompatibility of the implant. sex and integration.
Smart Images

Figure CN118084465B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of artificial eye base preparation, and in particular to a method for preparing a 3D printed porous bioceramic artificial eye base. Background Art
[0002] In cases of severe orbital injury, intraocular cancer and other life-threatening diseases, it is sometimes necessary to surgically remove the patient's damaged eye. Simple enucleation or evisceration of the eyeball often causes sunken upper tarsal grooves; lower eyelid margin sinking, artificial eye sinking, sluggish, and unable to rotate; even lower eyelid ectropion, disappearance of the lower fornix, and frequent slippage of the artificial eye. These symptoms can be collectively referred to as post-enucleation deformity syndrome, which imposes a heavy mental and psychological burden on patients, affects their social activities, and reduces their quality of life. Therefore, after the removal of the eye, an orbital implant is placed in the eyeless eye socket to provide adequate volume restoration and improve the appearance of the normal eye.
[0003] Currently, the most common artificial eye implants are divided into three categories according to the materials. The first category is the hydroxyapatite (HA) artificial eye scaffold. The HA artificial eye scaffold was approved by the FDA for marketing in 1989 and has the largest market share in my country. The problem is that the raw materials of HA are taken from natural corals. With the promulgation of the coral harvesting ban, the production cost of this product has been rising. The second is the high-density polyethylene Medpor (Porex surgical Inc., Newnan, GA) artificial eye scaffold. It has good mechanical strength, chemical stability and non-toxicity, and has been widely used in clinical practice as an intraorbital implant material. However, the Medpor material is highly hydrophobic and cannot provide a good biological interface for the attachment and growth of seed cells. Other experiments have shown that the vascularization rate of Medpor is slower than that of HA and alumina. Therefore, this product has defects in biocompatibility. The third category is the bioceramic alumina (Bioceramic, aluminum oxide, Al2O3) artificial eye scaffold, which is the lightest and has the lowest production cost among the three types of materials;
[0004] Bioceramic artificial eyes composed of alumina are implants with good biocompatibility and integration. Their safety is comparable to that of commonly used alternatives (such as hydroxyapatite and high-density polyethylene). Alumina has been widely used in orthopedics and dentures due to its durability and bioinertness. Its surface promotes the proliferation of fibroblasts, and when inserted into the body, the protein coating acts as an "immune camouflage" to promote its integration with orbital tissue. Alumina is a highly biocompatible material, so Al2O3 has a lower rate of secondary orbital inflammation and orbital exposure than HA and Medpor, and recent studies have also shown that postoperative exposure of alumina orbital implants can be repaired.
[0005] The use of 3D printing to prepare alumina artificial eye sockets can design the shape of the artificial eye sockets according to different conditions of the patients. At the same time, the use of 3D printing technology can control the aperture size and aperture direction compared to the template method, which is conducive to the attachment and growth of fibrous tissue in the artificial eye socket. Tarjani, Vivek Dave and others used 3D printing to prepare implants for correcting right eye socket migration, using computed tomography (CT) to scan the details inside the orbit, and printed suitable implants according to different orbital shapes. Jenny, Jarry and others used 3D printed orbital implants and implanted them into the horse's eye. The experimental results showed that there was soft tissue covering the inside of the implant, proving that the use of 3D printed artificial eye sockets is feasible. Therefore, the present invention proposes a method for preparing a 3D printed porous bioceramic artificial eye socket. Summary of the invention
[0006] In view of the above problems, the present invention proposes a method for preparing a 3D printed porous bioceramic artificial eye base. The method for preparing a 3D printed alumina porous bioceramic artificial eye base comprises preparing alumina, and then using alumina and pseudo-boehmite as raw materials respectively, controlling the processing environment, and then printing the artificial eye base through 3D printing technology.
[0007] To achieve the purpose of the present invention, the present invention is implemented by the following technical scheme: a preparation method of a 3D printed porous bioceramic artificial eye base, which is made by the following steps;
[0008] S1. Preparing pseudo-boehmite powder: using aluminum isopropoxide, deionized water and isopropanol as raw materials, wherein the ratio of aluminum isopropoxide to isopropanol to deionized water is 1:1:4, and then heating and stirring to obtain pseudo-boehmite colloid, centrifuging the colloid using a centrifuge, placing the centrifuged colloid in an oven for drying, and grinding the dried solid in an agate mortar to obtain pseudo-boehmite powder;
[0009] S2, performing 3D printing using pseudo-boehmite powder as a precursor, passing the obtained pseudo-boehmite powder through a 400-mesh sieve, and then adding a PVA binder to prepare a printing ink;
[0010] S3, dissolving polycaprolactone in chloroform, and then adding aluminum isopropoxide to prepare support ink for printing support materials;
[0011] S4. Use SOLIDWORKS software to design a 3D model with a spherical or egg-shaped shape, preset a surgical threading tunnel at the lower end of the sphere or egg-shaped shape, the diameter of the sphere is 18-22 mm, and the ratio of the long diameter to the short diameter of the egg-shaped shape is 1.35. Save the STL format and import it into the printing software for slicing;
[0012] S5, respectively loading the printing ink and the supporting ink into the printing chamber 1 and the printing chamber 2 of the 3D-Bioplotter, selecting a conical PP dispensing needle, squeezing out the ink at a certain speed under a certain gas pressure, and stacking layer by layer to obtain a finished product that conforms to the model, and controlling the pore structure and pore size by controlling the printing speed, printing layer thickness, printing route and filling spacing;
[0013] S6. Place the printed sphere or ellipsoid in a dry place for 24 hours of drying, place it in a tube furnace for sintering, and then cool it to room temperature;
[0014] S7. Gently rub the support material to remove it, and use sandpaper to polish the rough areas on the surface of the artificial eye.
[0015] Further improvements are: in step S1, the temperature during heating and stirring is 55°C, the reaction time is 5 hours, the centrifugal speed of the centrifuge during centrifugation is 10000r / min, the centrifugation time is 10 minutes, and the drying temperature during drying is 60°C and the time is 12 hours.
[0016] A further improvement is that in step S2, 5 g of polyvinyl alcohol is mixed with 45 ml of deionized water, stirred on a heated stirring table at 95° C. for 5 h, and cooled to room temperature to obtain a PVA adhesive.
[0017] A further improvement is that in step S2, the ratio of pseudo-boehmite powder to PVA is 1:0.9.
[0018] A further improvement is that in step S3, the ratio of chloroform to polycaprolactone to aluminum isopropoxide is 2.86:0.83:1.2.
[0019] Further improvements are: in step S5, the dispensing needle used is 20G-22G, the air pressure of printing chamber 1 is 1-2.4Mpa, the air pressure of printing chamber 2 is 1-5Mpa, and the printing speed is 3mm / min-8mm / min.
[0020] A further improvement is that in step S6, the sintering temperature in the tubular furnace is first raised to 1500°C at 4°C / min, then cooled to 1450°C at 5°C / min, and kept at this temperature for 4 hours.
[0021] The beneficial effects of the present invention are as follows: the present invention adopts an aluminum isopropoxide hydrolysis method to prepare an alumina bioceramic, which has the characteristics of low density, wear resistance, high stability and good biocompatibility. The SOLIDWORKS software is used to design a suitable model in combination with the orbital details of computer tomography (CT), and then the 3D printing technology is used to obtain the most suitable implant, and the speed is faster and the cost is lower than that of the template method. At the same time, the pore structure and pore size are controlled by controlling the printing speed, printing layer thickness, printing route and filling spacing, which is more conducive to the growth of fibrous tissue and reduces the exposure rate of the implant. The density of the artificial eye base printed with pseudo-boehmite powder is lower than that of the artificial eye base printed with α-alumina, and the porosity is higher. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 Flow chart of the method of the present invention.
[0023] Figure 2 This is a sample picture of the alumina artificial eye mount prepared by the method of the present invention.
[0024] Figure 3 This is a scanning electron microscope image of the alumina artificial eye platform prepared by the method of the present invention.
[0025] Figure 4 This is the XRD analysis diagram of the α-alumina component prepared by the method of the present invention.
[0026] Figure 5 This is the XRD analysis diagram of the pseudo-boehmite composition prepared by the method of the present invention. DETAILED DESCRIPTION
[0027] In order to deepen the understanding of the present invention, the present invention will be further described in detail below in conjunction with examples. The examples are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention. Embodiment 1
[0028] according to Figure 1-3 As shown, this embodiment proposes a method for preparing a 3D printed porous bioceramic artificial eye base.
[0029] (1) Take 10 g of aluminum isopropoxide (analytical grade) and mix it with 40 ml of deionized water to prepare a solution. Then add 10 ml of isopropanol (analytical grade) to the solution and stir it on a heated stirring table at 55°C and 600 r / min for 5 hours to obtain pseudo-boehmite colloid.
[0030] (2) Place the colloid in a centrifuge and centrifuge at 10,000 r / min for 10 minutes. Remove the supernatant and take out the solid and dry it in a 60°C oven for 12 hours.
[0031] (3) The dried white block is ground into pseudo-boehmite powder, which is then placed in a tube furnace and calcined at 1200°C for 4 hours to obtain alumina powder.
[0032] (4) Mix 5 g of polyvinyl alcohol with 45 ml of deionized water, stir on a heated stirring table at 95 °C for 5 h, and cool to room temperature to obtain a PVA solution as a binder.
[0033] (5) Mix 1.2 g of α-alumina powder (passing 400 mesh) with 1 ml of PVA solution to obtain a white slurry as printing ink. Load the printing ink into the printing chamber 1 of the 3D-Bioplotter and squeeze out the bubbles in the slurry. Use a 22G conical PP dispensing needle to mix 0.83 g of polycaprolactone with 2.86 ml of chloroform and place it in a 37°C oven for 2 h to obtain a transparent colloidal liquid. Add 1 ml of PVA solution to the colloidal liquid and mix thoroughly. Then add 1.2 g of aluminum isopropoxide and stir evenly to obtain the supporting ink. Load the supporting ink into the printing chamber 2 of the 3D-Bioplotter and squeeze out the bubbles in the slurry. Use a 22G conical PP dispensing needle.
[0034] (6) Use SOLIDWORKS software to design a series of 3D models with spherical or egg shapes. Preset surgical suture tunnels at the lower ends of the spheres and eggs to facilitate surgical suturing. The diameter of the sphere is 18-22 mm, and the ratio of the long to short diameter of the egg is 1.35. Save the model in STL format and import it into the printing software for slicing.
[0035] (7) During the printing process, the air pressure in printing chamber 1 is 1.4 MPa, the needle speed is 2.5 mm / s, the thickness of each layer is 0.33 mm, and the filling spacing is 0.4 mm. The air pressure in printing chamber 2 is 1.8 MPa, the needle speed is 4.5 mm / s, the thickness of each layer is 0.32 mm, and the filling spacing is 0.13 mm.
[0036] (8) Place the printed sphere or ellipsoid in a dry place for 24 hours. After drying, place it in a tubular furnace for sintering. Raise the temperature to 1500°C at 4°C / min, then cool it to 1450°C at 5°C / min and keep it at that temperature for 4 hours. Then cool it to room temperature to remove the binder and form the α-Al2O3 artificial eye platform.
[0037] (9) Gently rub the support material to remove it, and then use sandpaper to polish the rough areas on the surface of the artificial eye.
[0038] Density and porosity analysis revealed that its density was 1.01g / cm3 and its porosity was 80.65%. Embodiment 2
[0039] (1) Take 10 g of aluminum isopropoxide (analytical grade) and mix it with 40 ml of deionized water to prepare a solution. Then add 10 ml of isopropanol (analytical grade) to the solution and stir it on a heated stirring table at 55°C and 600 r / min for 5 hours to obtain pseudo-boehmite colloid.
[0040] (2) Place the colloid in a centrifuge and centrifuge at 10,000 r / min for 10 minutes. Remove the supernatant and take out the solid and dry it in a 60°C oven for 12 hours.
[0041] (3) Grind the dried white block to obtain pseudo-boehmite powder.
[0042] (4) Mix 2 g of pseudo-boehmite powder (passed through 400 mesh) with 1.8 ml of PVA solution to obtain a milky white slurry as ink. Load the ink into the printing chamber 1 of the 3D-Bioplotter and squeeze out the bubbles in the slurry. Use a 22G conical PP dispensing needle.
[0043] (5) Mix 0.83 g of polycaprolactone with 2.86 ml of chloroform and place in a 37 °C oven for 2 h to obtain a transparent colloidal liquid. Add 1 ml of PVA solution to the colloidal liquid and mix thoroughly. Then add 1.2 g of aluminum isopropoxide and stir evenly. Load the obtained slurry into the printing chamber 2 of the 3D-Bioplotter and squeeze out the bubbles in the slurry. Use a 22G conical PP dispensing needle as the support material.
[0044] (6) Use SOLIDWORKS software to design a series of 3D models with spherical or egg shapes. Preset surgical suture tunnels at the lower end of the sphere or egg shape to facilitate surgical suturing. The diameter of the sphere is 18-22 mm, and the ratio of the long to short diameter of the egg shape is 1.35. Save the model in STL format and import it into the printing software for slicing.
[0045] (7) The air pressure of printing chamber 1 is 2.4Mpa, the speed of the needle is 3.5mm / s, the thickness of each layer is 0.32mm, and the filling spacing is 0.15mm. The air pressure of printing chamber 2 is 1.8Mpa, the speed of the needle is 4.5mm / s, the thickness of each layer is 0.32mm, and the filling spacing is 0.13mm.
[0046] (8) Place the printed sphere or ellipsoid in a dry place for 24 hours. After drying, place it in a tubular furnace for sintering. Raise the temperature to 1500°C at 4°C / min, then cool it to 1450°C at 5°C / min and keep it at that temperature for 4 hours. Then cool it to room temperature to remove the binder and form the α-Al2O3 artificial eye base.
[0047] (9) Gently rub the support material to remove it, and use sandpaper to polish the rough areas on the surface of the artificial eye.
[0048] Density and porosity analysis revealed that its density was 0.87g / cm3 and its porosity was 85.22%.
[0049] The alumina powder and pseudo-boehmite powder prepared in the above-mentioned Example 1 and Example 2 were subjected to X-ray diffraction (XRD) component analysis, and the surface morphology of the alumina artificial eye stage was analyzed by scanning electron microscopy (SEM);
[0050] The results of the above samples are analyzed as follows:
[0051] 1. XRD analysis of alumina powder Figure 4 As shown, it can be seen that the diffraction peaks of the aluminum oxide powder all appear, there are no other impurity peaks, and it has high crystallinity.
[0052] 2. XRD analysis of pseudo-boehmite powder Figure 5 As shown, it can be seen that the diffraction peaks of pseudo-boehmite all correspond, but the diffraction peaks are not sharp because the crystallinity of pseudo-boehmite is general.
[0053] 3. SEM analysis results of alumina artificial eye base Figure 3 As shown, it can be seen that α-alumina forms a worm-like and lamellar structure when sintered at 1500°C, showing that the grains are not fully grown. Embodiment 3
[0054] The effect of temperature on alumina artificial eye sockets (700-1500℃) (porosity and density);
[0055] (1) Prepare spheres or ellipsoids using (1) to (7) in Example 2 and dry them for 24 hours.
[0056] (2) The dried sample was placed in a tube furnace and heated to 700°C at 4°C / min, and then cooled to room temperature.
[0057] Density and porosity analysis revealed that its density was 1.18 g / cm3 and its porosity was 76.81%. Embodiment 4
[0058] About the effect of different printing conditions (air pressure) on (porosity and density);
[0059] (1) The steps in Example 2 are used, but the air pressure of the printing chamber 1 is 3.2 MPa and the speed of the needle is 5.5 mm / s.
[0060] Density and porosity analysis revealed that its density was 1.04g / cm3 and its porosity was 72.23%. Embodiment 5
[0061] About the effect of different binders on printing results (porosity and density);
[0062] (1) The difference from Example 2 is that the binder used in the printing chamber 1 is changed to chloroform and polycaprolactone (PCL). 0.8 g PCL and 3 mL chloroform are placed in a 37°C oven for 20 min, and then 3.2 g of pseudo-boehmite powder passed through a 400-mesh sieve is fully mixed with them.
[0063] Density and porosity analysis revealed that its density was 1.12 g / cm3 and its porosity was 73.78%. Embodiment 6
[0064] The difference from Example 2 is that the binder used in the printing chamber 1 is changed to chloroform and L-polylactic acid (PLLA), 0.75g PLLA and 3mL chloroform are placed in a 60°C oven for 2h, and then 3g of pseudo-boehmite powder passed through a 400-mesh sieve is fully mixed with it.
[0065] Density and porosity analysis revealed that its density was 1.98 g / cm3 and its porosity was 62.38%.
[0066] The results of the above examples are analyzed as follows:
[0067] Using pseudo-boehmite as the raw material, the artificial eye base obtained has the lowest density, higher porosity and better effect. At the same time, the hardness of pseudo-boehmite is lower than that of alumina, which can save more time during grinding. And because pseudo-boehmite is easily soluble in water, it is easily soluble in PVA solution, and the resulting slurry is more uniform, the printing effect is better, and the surface is smoother.
[0068] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing a 3D printed porous bioceramic artificial eye base, characterized in that: Made by following the steps below: S1. Preparing pseudo-boehmite powder: using aluminum isopropoxide, deionized water and isopropanol as raw materials, wherein the ratio of aluminum isopropoxide to isopropanol to deionized water is 1:1:4, and then heating and stirring to obtain pseudo-boehmite colloid, centrifuging the colloid using a centrifuge, placing the centrifuged colloid in an oven for drying, and grinding the dried solid in an agate mortar to obtain pseudo-boehmite powder; S2. Performing 3D printing using pseudo-boehmite powder as a precursor: passing the obtained pseudo-boehmite powder through a 400-mesh sieve, and then adding a PVA binder to prepare a printing ink; S3, dissolving polycaprolactone in chloroform and then adding aluminum isopropoxide to prepare support ink for printing support materials; S4. Use SOLIDWORKS software to design a 3D model with a spherical or egg-shaped shape, preset a surgical threading tunnel at the lower end of the sphere or egg-shaped shape, the diameter of the sphere is 18-22 mm, and the ratio of the long diameter to the short diameter of the egg-shaped shape is 1.
35. Save the STL format and import it into the printing software for slicing; S5, respectively loading the printing ink and the supporting ink into the printing chamber 1 and the printing chamber 2 of the 3D-Bioplotter, selecting a conical PP dispensing needle, squeezing out the ink at a certain speed under a certain gas pressure, and stacking layer by layer to obtain a finished product that conforms to the model, and controlling the pore structure and pore size by controlling the printing speed, printing layer thickness, printing route and filling spacing; S6. Place the printed sphere or ellipsoid in a dry place for 24 hours of drying, place it in a tube furnace for sintering, and then cool it to room temperature; S7. Gently rub the support material to remove it, and use sandpaper to polish the rough areas on the surface of the artificial eye. In step S1, the temperature during heating and stirring is 55° C., the reaction time is 5 h, the centrifugal speed of the centrifuge during centrifugation is 10000 r / min, the centrifugal time is 10 min, and the drying temperature during drying is 60° C., and the time is 12 h; In step S2, 5 g of polyvinyl alcohol was mixed with 45 ml of deionized water, stirred at 95° C. for 5 h on a heated stirring table, and cooled to room temperature to obtain a PVA adhesive; In step S2, the ratio of pseudo-boehmite powder to PVA is 1:0.9; In step S3, the ratio of chloroform to polycaprolactone to aluminum isopropoxide is 2.86:0.83:1.2; In step S5, the dispensing needle used is 20G-22G, the air pressure of printing chamber 1 is 1-2.4Mpa, the air pressure of printing chamber 2 is 1-5Mpa, and the printing speed is 3mm / min-8mm / min; In step S6, the sintering temperature in the tubular furnace is first raised to 1500° C. at 4° C. / min, then cooled to 1450° C. at 5° C. / min, and kept at this temperature for 4 hours.
Citation Information
Patent Citations
Three-dimensional printing molding preparation method for porous ceramic for filtration
CN107098717A
Individualized 3D printing multifunctional artificial orbital implant and preparation method thereof
CN109087387A
Catalyst alumina carrier material with gradient structure and preparation method thereof
CN112827481A