Aluminum-copper-iron-boron quaternary quasicrystal-silicon carbide coating and preparation method thereof
By adding boron elements to aluminum, copper, iron, teremicromethic crystals and mixing them with silicon carbide, the aluminum, copper, iron, boron quasi-crystals-silicon carbide coating was prepared, which solved the problem of large porosity of traditional coatings and improved the titanium alloy. Wear resistance has expanded its industrial applications.
Patent Information
- Application Number
- CN202410890459.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional quasicrystal coatings have a high porosity on titanium alloy materials, which cannot effectively improve the wear resistance of titanium alloys, limiting its industrial applications.
Boron elements are added on the basis of aluminum, copper, iron and iron ternary quasi-crystals, aluminum, copper, iron and boron quasi-crystals are prepared by aerosolization method and silicon carbide powder are prepared, and aluminum, copper, iron and iron and boron quasi-crystals are prepared by hypersonic flame spraying technology. -Silicon carbide coating, as surface protective coating for titanium alloy.
It significantly reduces the porosity of the coating, improves hardness, significantly improves the wear resistance of titanium alloy materials, and expands its industrial applications.
Smart Images

Figure CN118957480A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of quasi-crystal-silicon carbide coating preparation, and specifically relates to an aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating and a preparation method thereof. Background Art
[0002] As an important lightweight structural material, titanium alloy is widely used in aviation and other fields due to its low density, good heat and corrosion resistance, and high mechanical properties. However, due to problems such as poor wear resistance, titanium alloy is limited in its application in more fields.
[0003] Compared with metal alloys, aluminum-based quasicrystal materials have the characteristics of low surface energy, low friction coefficient, wear resistance, high hardness, and corrosion resistance. However, due to their intrinsic brittleness, quasicrystal materials are not easy to be used alone as structural parts and are often used as surface protective coatings. However, traditional quasicrystal coatings have the disadvantage of large porosity. Applying traditional quasicrystal coatings to titanium alloy materials does not help to effectively solve the problem of poor wear resistance of titanium alloys, and the limitations of industrial applications of titanium alloys still exist. Summary of the invention
[0004] The purpose of the present invention is to provide an aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating and a preparation method thereof in view of the background technology so as to solve the technical problems existing in the prior art.
[0005] The basic technical concept of the present invention is to add the fourth component boron element to the aluminum-copper-iron ternary quasicrystal and prepare the aluminum-copper-iron-boron quaternary quasicrystal Al by gas atomization method. 59 Cu 25 Fe 12.6 B 3.4 , then Al 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasicrystal is mixed with SiC and then sprayed on a titanium alloy substrate, thereby preparing an aluminum-copper-iron-boron quaternary quasicrystal-silicon carbide coating, which is used as a surface protective coating for the titanium alloy to improve the wear resistance of the titanium alloy substrate material.
[0006] The aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating provided by the present invention comprises Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasi-crystal powder and silicon carbide powder, the Al 59 Cu 25 Fe 12.6 B 3.4 The mass ratio of the quaternary quasicrystal powder to the silicon carbide powder is 1:2. 59 Cu 25 Fe 12.6 B3.4 The quaternary quasi-crystal powder and the silicon carbide powder are spherical powders with a particle size of ≤45 μm. 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasi-crystal powder contains the following components in percentage by mass: 40-41% of aluminum powder, 41-42% of copper powder, 17-18% of iron powder, and 0.7-0.9% of boron powder.
[0007] The method for preparing the aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating provided by the present invention comprises:
[0008] 1. Powder preparation
[0009] (1) Weigh aluminum powder, copper powder, iron powder and boron powder according to the following mass percentages: 40-41% aluminum powder, 41-42% copper powder, 17-18% iron powder, and 0.7-0.9% boron powder;
[0010] (2) Pour the weighed aluminum powder, copper powder, iron powder and boron powder into a vacuum drying oven for drying, the drying temperature is controlled at 190-210° C., the drying time is controlled at 110-130 min, and the vacuum degree is 1.8-2.2 Pa;
[0011] 2. Aerosolization
[0012] (1) introducing the dried aluminum powder, copper powder, iron powder and boron powder into a melting crucible of a magnetic levitation vacuum melting furnace;
[0013] (2) closing and sealing the magnetic levitation vacuum melting furnace, and using the vacuum pump in the vacuum melting furnace to extract the air in the furnace to make the pressure in the furnace reach 1 Pa;
[0014] (3) Turn on the argon device of the magnetic levitation vacuum melting furnace, input argon into the furnace and adjust the pressure in the furnace through the outlet valve of the vacuum melting furnace. The argon delivery speed is controlled to 240-260 cm 3 / min, and keep the pressure in the furnace constant at 1Pa;
[0015] (4) Turn on the heater of the magnetic levitation vacuum melting furnace to heat, and control the heating temperature to 950°C ± 1°C, and melt the aluminum powder, copper powder, iron powder and boron powder into a melt. When the melt temperature reaches 950°C ± 1°C, keep it warm for 2.5 to 3.5 minutes;
[0016] (5) The melt was atomized using argon gas with a purity of 99.999% and the atomization pressure was controlled at 2.5±0.1 MPa to atomize the melt into droplets and then solidify into powder to obtain Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder;
[0017] 3. Screening and mixing powder
[0018] (1) Use a 45 μm standard mesh to screen Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder;
[0019] (2) Silicate the silicon carbide powder using a 45 μm standard mesh sieve;
[0020] (3) The screened Al 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasicrystal powder and silicon carbide powder are mixed in a mass ratio of 1:2 and then put into a planetary ball mill for mixing. The ball mill speed is controlled at 190-210 r / min and the mixing time is controlled at 9-11 min.
[0021] 4. Prepare the base material
[0022] The surface of the titanium alloy block as the base material is polished with sandpaper, and the surface of the titanium alloy block is cleaned with acetone solution;
[0023] 5. Use hypersonic flame spraying equipment for spraying
[0024] (1) Clamp the titanium alloy block, adjust the distance between the spray gun of the hypersonic flame spraying equipment and the titanium alloy block to 170-190 mm, and keep the spray gun parallel to the titanium alloy block;
[0025] (2) pouring corundum powder into a powder feeder of a hypersonic flame spraying device, turning on the powder feeder, and using the corundum powder in the powder feeder to sandblast the titanium alloy block;
[0026] (3) Turn off the powder feeder, pour out the corundum powder, and pour in the mixed Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder and silicon carbide powder;
[0027] (4) Start the spray gun, set the horizontal speed of the spray gun to 1200mm / s±10mm / s, the power of the spray gun to 200kw±1kw, the pressure of the spray gun to 437.8Kpa±0.1Kpa, the oxygen-fuel ratio to 94:76, start the powder feeder, control the powder feeding rate of the powder feeder to 3r / min, and start the first spraying;
[0028] (5) After the first spraying, the distance between the spray gun and the titanium alloy block is adjusted to 190-210 mm, the horizontal movement speed of the spray gun is adjusted to 800 mm / s±10 mm / s, the powder feeding rate is adjusted to 5 r / min, and the second spraying is carried out;
[0029] (6) After the second spraying, the horizontal movement speed of the spray gun is adjusted to 1200 mm / s±10 mm / s, and the third spraying is performed, thereby preparing an aluminum-copper-iron-boron quasi-crystal-silicon carbide coating.
[0030] As a specific embodiment, the chemical materials used in the method for preparing the aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating of the present invention are: aluminum powder, iron powder, copper powder, boron powder, argon, nitrogen, silicon carbide powder, hydrogen, corundum, and the combined preparation amounts thereof are as follows:
[0031]
[0032] The specific preparation method includes:
[0033] 1) Prepare powder
[0034] 1.1) Select 200 mesh aluminum powder, copper powder, iron powder and boron powder;
[0035] 1.2) Weigh 120.7g±0.1g of aluminum powder, 123.7g±0.1g of copper powder, 53.0g±0.1g of iron powder, and 2.5g±0.1g of boron powder, and put the weighed aluminum powder, copper powder, iron powder, and boron powder into a vacuum drying oven for drying at a temperature of 200°C, a drying time of 120min, and a vacuum degree of 2Pa;
[0036] 2) Aerosolization
[0037] 2.1) Open the magnetic levitation vacuum melting furnace and clean the melting crucible of the vacuum melting furnace to ensure that the residual powder in the atomization chamber does not contaminate subsequent new products;
[0038] 2.2) introducing the dried aluminum powder, copper powder, iron powder and boron powder into a smelting crucible;
[0039] 2.3) The magnetic suspension vacuum melting furnace is closed and sealed, and then the vacuum pump in the vacuum melting furnace is used to extract the air in the furnace to make the pressure in the furnace reach 1Pa;
[0040] 2.4) Turn on the argon device of the magnetic levitation vacuum melting furnace, input argon into the furnace and adjust the pressure in the furnace through the outlet valve of the vacuum melting furnace. The argon delivery speed is 250cm 3 / min, and keep the pressure in the furnace constant at 1Pa;
[0041] 2.5) Turn on the heater of the magnetic levitation vacuum melting furnace to heat at a temperature of 950°C ± 1°C, melt the aluminum powder, copper powder, iron powder and boron powder into a melt, and when the melt temperature reaches 950°C ± 1°C, keep it warm for 3 minutes;
[0042] 2.6) Start atomization, use argon gas with a purity of 99.999% to gas atomize the melt, and the atomization pressure is 2.5±0.1MPa, thereby atomizing the melt into droplets and then solidifying into powder to obtain Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder;
[0043] 3) Screening and mixing powders
[0044] 3.1) First use a 65μm standard mesh to filter Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasi-crystal powder, and then Al 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasicrystal powder was screened with a 45 μm standard mesh;
[0045] 3.2) Sifting silicon carbide powder with a 45 μm standard mesh;
[0046] 3.3) The screened Al 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasicrystal powder and silicon carbide powder were mixed in a mass ratio of 1:2 and then placed in a planetary ball mill for mixing. The ball mill speed was 200 r / min and the mixing time was 10 min.
[0047] 4) Prepare the base material
[0048] 4.1) Cut the TC4 titanium alloy into titanium alloy blocks with a size of 50 mm × 50 mm × 10 mm using a block cutter;
[0049] 4.2) Use 800-grit sandpaper to polish the surface of the titanium alloy block to make it bright;
[0050] 4.3) Cleaning the surface of the titanium alloy block with acetone solution;
[0051] 5) Use hypersonic flame spraying equipment for spraying
[0052] 5.1) Clamp the titanium alloy block with a mold;
[0053] 5.2) Adjust the distance between the spray gun of the hypersonic flame spraying equipment and the titanium alloy block to 180 mm, and keep the spray gun parallel to the titanium alloy block;
[0054] 5.3) Start the air compressor of the hypersonic flame spraying equipment to backflush the spraying room to keep it clean;
[0055] 5.4) Start the hypersonic flame spraying equipment and preheat the titanium alloy block 10 times;
[0056] 5.5) Pour the corundum powder into the powder feeder of the hypersonic flame spraying equipment, turn on the powder feeder, and use the corundum powder in the powder feeder to sandblast the titanium alloy block, sandblasting twice;
[0057] 5.6) Turn off the powder feeder, pour out the corundum powder, and pour in the mixed Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder and silicon carbide powder;
[0058] 5.7) Start the spray gun, set the horizontal speed of the spray gun to 1200mm / s±10mm / s, the power of the spray gun to 200kw±1kw, the pressure of the spray gun to 437.8Kpa±0.1Kpa, the oxygen-fuel ratio to 94:76, and after the sound of the spray gun becomes stable, start the powder feeder with a powder feed rate of 3r / min. When the flame of the spray gun changes from blue to red, start the first spraying;
[0059] 5.8) After the first spraying, the distance between the spray gun and the titanium alloy block is adjusted to 200mm, the horizontal movement speed of the spray gun is adjusted to 800mm / s±10mm / s, the powder feeding rate is adjusted to 5r / min, and the other parameters are consistent with the parameters of the first spraying, and the second spraying is carried out;
[0060] 5.9) After the second spraying, the horizontal movement speed of the spray gun is adjusted to 1200 mm / s±10 mm / s, and the other parameters are consistent with the parameters of the second spraying, and the third spraying is carried out to prepare the aluminum-copper-iron-boron quasi-crystal-silicon carbide coating.
[0061] 6) Detection, analysis, and characterization
[0062] The morphology of the prepared aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating was analyzed using a scanning electron microscope, and the XRD analysis of the prepared aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating was performed using an X-ray diffractometer.
[0063] The aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating and the preparation method thereof of the present invention have the following advantages and beneficial effects: the present invention combines the advantages of low surface energy, low friction coefficient, wear resistance, high hardness, corrosion resistance of aluminum-based crystal materials and low price and high wear resistance of silicon carbide. The porosity of the prepared aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating is effectively reduced and the hardness is significantly improved, thus solving the problem of high porosity of traditional quasi-crystal coatings. The coating is applied to titanium alloys, which can significantly improve the wear resistance of titanium alloy materials and effectively expand the industrial application of titanium alloys. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work. In the drawings:
[0065] Figure 1 This is a surface morphology diagram of the aluminum-copper-iron-boron quasi-crystal-silicon carbide coating of the present invention. DETAILED DESCRIPTION
[0066] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0067] The aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating of the present invention comprises Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder and silicon carbide powder, Al 59 Cu 25 Fe 12.6 B 3.4 The mass ratio of quaternary quasicrystal powder to silicon carbide powder is 1:2. 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasi-crystal powder and silicon carbide powder are spherical powders with a particle size of ≤45μm. 59 Cu 25 Fe 12.6 B 3.4The quaternary quasi-crystal powder contains the following components in percentage by mass: 40-41% of aluminum powder, 41-42% of copper powder, 17-18% of iron powder, and 0.7-0.9% of boron powder.
[0068] As known to those skilled in the art, the term “Al” herein refers to 59 Cu 25 Fe 12.6 B 3.4 "The subscript numbers of the elements in the formula represent Al 59 Cu 25 Fe 12.6 B 3.4 The element molar ratio of Al:Cu:Fe:B in the quaternary quasicrystal is 59:25:12.6:3.4.
[0069] The method for preparing the aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating of the present invention comprises:
[0070] 1. Powder preparation
[0071] (1) Weigh aluminum powder, copper powder, iron powder and boron powder according to the following mass percentages: 40-41% aluminum powder, 41-42% copper powder, 17-18% iron powder, and 0.7-0.9% boron powder;
[0072] (2) Pour the weighed aluminum powder, copper powder, iron powder and boron powder into a vacuum drying oven for drying, the drying temperature is controlled at 190-210° C., the drying time is controlled at 110-130 min, and the vacuum degree is 1.8-2.2 Pa;
[0073] 2. Aerosolization
[0074] (1) introducing the dried aluminum powder, copper powder, iron powder and boron powder into a melting crucible of a magnetic levitation vacuum melting furnace;
[0075] (2) closing and sealing the magnetic levitation vacuum melting furnace, and using the vacuum pump in the vacuum melting furnace to extract the air in the furnace to make the pressure in the furnace reach 1 Pa;
[0076] (3) Turn on the argon device of the magnetic levitation vacuum melting furnace, input argon into the furnace and adjust the pressure in the furnace through the outlet valve of the vacuum melting furnace. The argon delivery speed is controlled to 240-260 cm 3 / min, and keep the pressure in the furnace constant at 1Pa;
[0077] (4) Turn on the heater of the magnetic levitation vacuum melting furnace to heat, and control the heating temperature to 950°C ± 1°C, and melt the aluminum powder, copper powder, iron powder and boron powder into a melt. When the melt temperature reaches 950°C ± 1°C, keep it warm for 2.5 to 3.5 minutes;
[0078] (5) The melt was atomized using argon gas with a purity of 99.999% and the atomization pressure was controlled at 2.5±0.1 MPa to atomize the melt into droplets and then solidify into powder to obtain Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder;
[0079] 3. Screening and mixing powder
[0080] (1) Use a 45 μm standard mesh to screen Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder;
[0081] (2) Silicate the silicon carbide powder using a 45 μm standard mesh sieve;
[0082] (3) The screened Al 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasicrystal powder and silicon carbide powder are mixed in a mass ratio of 1:2 and then put into a planetary ball mill for mixing. The ball mill speed is controlled at 190-210 r / min and the mixing time is controlled at 9-11 min.
[0083] 4. Prepare the base material
[0084] The surface of the titanium alloy block as the base material is polished with sandpaper, and the surface of the titanium alloy block is cleaned with acetone solution;
[0085] 5. Use hypersonic flame spraying equipment for spraying
[0086] (1) Clamp the titanium alloy block, adjust the distance between the spray gun of the hypersonic flame spraying equipment and the titanium alloy block to 170-190 mm, and keep the spray gun parallel to the titanium alloy block;
[0087] (2) pouring corundum powder into a powder feeder of a hypersonic flame spraying device, turning on the powder feeder, and using the corundum powder in the powder feeder to sandblast the titanium alloy block;
[0088] (3) Turn off the powder feeder, pour out the corundum powder, and pour in the mixed Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder and silicon carbide powder;
[0089] (4) Start the spray gun, set the horizontal speed of the spray gun to 1200mm / s±10mm / s, the power of the spray gun to 200kw±1kw, the pressure of the spray gun to 437.8Kpa±0.1Kpa, the oxygen-fuel ratio to 94:76, start the powder feeder, control the powder feeding rate of the powder feeder to 3r / min, and start the first spraying;
[0090] (5) After the first spraying, the distance between the spray gun and the titanium alloy block is adjusted to 190-210 mm, the horizontal movement speed of the spray gun is adjusted to 800 mm / s±10 mm / s, the powder feeding rate is adjusted to 5 r / min, and the second spraying is carried out;
[0091] (6) After the second spraying, the horizontal movement speed of the spray gun is adjusted to 1200 mm / s±10 mm / s, and the third spraying is performed, thereby preparing an aluminum-copper-iron-boron quasi-crystal-silicon carbide coating.
[0092] The specific embodiment of the method for preparing the aluminum-copper-iron-boron quasi-crystal-silicon carbide coating of the present invention is described in detail below.
[0093] Example 1
[0094] The chemical materials used in the method for preparing the aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating of Example 1 of the present invention are: aluminum powder, iron powder, copper powder, boron powder, argon, nitrogen, silicon carbide powder, hydrogen, corundum, and the combined preparation amounts thereof are as follows:
[0095]
[0096] The specific preparation method includes:
[0097] 1) Prepare powder
[0098] 1.1) Select 200 mesh aluminum powder, copper powder, iron powder and boron powder;
[0099] 1.2) Weigh 120.7g±0.1g of aluminum powder, 123.7g±0.1g of copper powder, 53.0g±0.1g of iron powder, and 2.5g±0.1g of boron powder, and put the weighed aluminum powder, copper powder, iron powder, and boron powder into a vacuum drying oven for drying at a temperature of 200°C, a drying time of 120min, and a vacuum degree of 2Pa;
[0100] 2) Aerosolization
[0101] 2.1) Open the magnetic levitation vacuum melting furnace and clean the melting crucible of the vacuum melting furnace to ensure that the residual powder in the atomization chamber does not contaminate subsequent new products;
[0102] 2.2) introducing the dried aluminum powder, copper powder, iron powder and boron powder into a smelting crucible;
[0103] 2.3) The magnetic suspension vacuum melting furnace is closed and sealed, and then the vacuum pump in the vacuum melting furnace is used to extract the air in the furnace to make the pressure in the furnace reach 1Pa;
[0104] 2.4) Turn on the argon device of the magnetic levitation vacuum melting furnace, input argon into the furnace and adjust the pressure in the furnace through the outlet valve of the vacuum melting furnace. The argon delivery speed is 250cm 3 / min, and keep the pressure in the furnace constant at 1Pa;
[0105] 2.5) Turn on the heater of the magnetic levitation vacuum melting furnace to heat at a temperature of 950°C ± 1°C, melt the aluminum powder, copper powder, iron powder and boron powder into a melt, and when the melt temperature reaches 950°C ± 1°C, keep it warm for 3 minutes;
[0106] 2.6) Start atomization, use argon gas with a purity of 99.999% to gas atomize the melt, and the atomization pressure is 2.5±0.1MPa, thereby atomizing the melt into droplets and then solidifying into powder to obtain Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder;
[0107] 3) Screening and mixing powders
[0108] 3.1) First use a 65μm standard mesh to filter Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasi-crystal powder, and then Al 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasicrystal powder was screened with a 45 μm standard mesh;
[0109] 3.2) Sifting silicon carbide powder with a 45 μm standard mesh;
[0110] 3.3) The screened Al 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasicrystal powder and silicon carbide powder were mixed in a mass ratio of 1:2 and then placed in a planetary ball mill for mixing. The ball mill speed was 200 r / min and the mixing time was 10 min.
[0111] 4) Prepare the base material
[0112] 4.1) Cut the TC4 titanium alloy into titanium alloy blocks with a size of 50 mm × 50 mm × 10 mm using a block cutter;
[0113] 4.2) Use 800-grit sandpaper to polish the surface of the titanium alloy block to make it bright;
[0114] 4.3) Cleaning the surface of the titanium alloy block with acetone solution;
[0115] 5) Use hypersonic flame spraying equipment for spraying
[0116] 5.1) Clamp the titanium alloy block with a mold;
[0117] 5.2) Adjust the distance between the spray gun of the hypersonic flame spraying equipment and the titanium alloy block to 180 mm, and keep the spray gun parallel to the titanium alloy block;
[0118] 5.3) Start the air compressor of the hypersonic flame spraying equipment to backflush the spraying room to keep it clean;
[0119] 5.4) Start the hypersonic flame spraying equipment and preheat the titanium alloy block 10 times;
[0120] 5.5) Pour the corundum powder into the powder feeder of the hypersonic flame spraying equipment, turn on the powder feeder, and use the corundum powder in the powder feeder to sandblast the titanium alloy block, sandblasting twice;
[0121] 5.6) Turn off the powder feeder, pour out the corundum powder, and pour in the mixed Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder and silicon carbide powder;
[0122] 5.7) Start the spray gun, set the horizontal speed of the spray gun to 1200mm / s±10mm / s, the power of the spray gun to 200kw±1kw, the pressure of the spray gun to 437.8Kpa±0.1Kpa, the oxygen-fuel ratio to 94:76, and after the sound of the spray gun becomes stable, start the powder feeder, the powder feed rate of the powder feeder (i.e. the powder plate speed of the powder feeder) is 3r / min, and start the first spraying when the flame of the spray gun changes from blue to red;
[0123] 5.8) After the first spraying, the distance between the spray gun and the titanium alloy block is adjusted to 200mm, the horizontal movement speed of the spray gun is adjusted to 800mm / s±10mm / s, the powder feeding rate is adjusted to 5r / min, and the other parameters are consistent with the parameters of the first spraying, and the second spraying is carried out;
[0124] 5.9) After the second spraying, the horizontal movement speed of the spray gun is adjusted to 1200 mm / s±10 mm / s, and the other parameters are consistent with the parameters of the second spraying, and the third spraying is carried out to prepare the aluminum-copper-iron-boron quasi-crystal-silicon carbide coating.
[0125] 6) Detection, analysis, and characterization
[0126] The morphology of the prepared aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating was analyzed using a scanning electron microscope, and the XRD analysis of the prepared aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating was performed using an X-ray diffractometer.
[0127] Figure 1 The surface morphology of the aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating of the present invention is shown, and according to the analysis results, the Al prepared by the gas atomization method 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasicrystal powder has high sphericity and high quasicrystal content. The porosity of the aluminum-copper-iron-boron quaternary quasicrystal-silicon carbide coating prepared by the hypersonic flame spraying equipment is 0.12%, and the average microhardness of the coating is as high as 1250HV 0.3 Compared with traditional quasi-crystal coatings, the porosity of the aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating of the present invention is reduced by 1.12% and the hardness is increased by 50%.
[0128] In summary, the present invention adds the fourth component boron element to the aluminum-copper-iron ternary quasicrystal and prepares the aluminum-copper-iron-boron quaternary quasicrystal Al by gas atomization method. 59 Cu 25 Fe 12.6 B 3.4 , then Al 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasicrystal is mixed with silicon carbide and then sprayed on a titanium alloy substrate, thereby preparing an aluminum-copper-iron-boron quaternary quasicrystal-silicon carbide coating, which is used as a surface protective coating for the titanium alloy.
[0129] Compared with the prior art, the aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating and the preparation method thereof of the present invention have the following advantages and beneficial effects: the present invention combines the advantages of low surface energy, low friction coefficient, wear resistance, high hardness, corrosion resistance of aluminum-based crystal materials and low price and high wear resistance of silicon carbide. The porosity of the prepared aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating is effectively reduced and the hardness is significantly improved, which solves the problem of high porosity of traditional quasi-crystal coatings. The coating is applied to titanium alloys, which can significantly improve the wear resistance of titanium alloy materials and effectively expand the industrial application of titanium alloys.
[0130] It should be noted that, in this article, the term "comprise" or any other variation thereof is intended to cover non-exclusive inclusion, so that an article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such article or device.
[0131] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating, characterized in that: The aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating comprises Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasi-crystal powder and silicon carbide powder, the Al 59 Cu 25 Fe 12.6 B 3.4 The mass ratio of the quaternary quasicrystal powder to the silicon carbide powder is 1:
2. 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasi-crystal powder and the silicon carbide powder are spherical powders with a particle size of ≤45 μm. 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasi-crystal powder contains the following components in percentage by mass: 40-41% of aluminum powder, 41-42% of copper powder, 17-18% of iron powder, and 0.7-0.9% of boron powder.
2. A method for preparing an aluminum-copper-iron-boron quasi-crystal-silicon carbide coating, characterized in that: include:
1. Preparation of powder (1) Weigh aluminum powder, copper powder, iron powder and boron powder according to the following mass percentages: 40-41% aluminum powder, 41-42% copper powder, 17-18% iron powder, and 0.7-0.9% boron powder; (2) Pour the weighed aluminum powder, copper powder, iron powder and boron powder into a vacuum drying oven for drying, the drying temperature is controlled at 190-210° C., the drying time is controlled at 110-130 min, and the vacuum degree is 1.8-2.2 Pa; 2. Aerosolization (1) introducing the dried aluminum powder, copper powder, iron powder and boron powder into a melting crucible of a magnetic levitation vacuum melting furnace; (2) closing and sealing the magnetic levitation vacuum melting furnace, and using the vacuum pump in the vacuum melting furnace to extract the air in the furnace to make the pressure in the furnace reach 1 Pa; (3) Turn on the argon device of the magnetic levitation vacuum melting furnace, input argon into the furnace, and adjust the pressure in the furnace through the outlet valve of the vacuum melting furnace. The argon delivery speed is controlled to 240-260 cm3 / min, and the pressure in the furnace is constant at 1 Pa; (4) Turn on the heater of the magnetic levitation vacuum melting furnace to heat, and control the heating temperature to 950°C ± 1°C, and melt the aluminum powder, copper powder, iron powder and boron powder into a melt. When the melt temperature reaches 950°C ± 1°C, keep it warm for 2.5 to 3.5 minutes; (5) The melt was atomized using argon gas with a purity of 99.999% and the atomization pressure was controlled at 2.5±0.1 MPa to atomize the melt into droplets which were then solidified into powder to obtain Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder; 3. Screening and mixing powders (1) Use a 45 μm standard mesh to screen Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder; (2) Sifting silicon carbide powder using a 45 μm standard mesh sieve; (3) The screened Al 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasicrystal powder and silicon carbide powder are mixed in a mass ratio of 1:2 and then put into a planetary ball mill for mixing. The ball mill speed is controlled at 190-210 r / min and the mixing time is controlled at 9-11 min.
4. Prepare the base material The surface of the titanium alloy block as the base material is polished with sandpaper, and the surface of the titanium alloy block is cleaned with acetone solution; 5. Use hypersonic flame spraying equipment for spraying (1) Clamp the titanium alloy block, adjust the distance between the spray gun of the hypersonic flame spraying equipment and the titanium alloy block to 170-190 mm, and keep the spray gun parallel to the titanium alloy block; (2) pouring corundum powder into a powder feeder of a hypersonic flame spraying device, turning on the powder feeder, and using the corundum powder in the powder feeder to sandblast the titanium alloy block; (3) Turn off the powder feeder, pour out the corundum powder, and pour in the mixed Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder and silicon carbide powder; (4) Start the spray gun, set the horizontal speed of the spray gun to 1200mm / s±10mm / s, the power of the spray gun to 200kw±1kw, the pressure of the spray gun to 437.8Kpa±0.1Kpa, the oxygen-fuel ratio to 94:76, start the powder feeder, control the powder feeding rate of the powder feeder to 3r / min, and start the first spraying; (5) After the first spraying, the distance between the spray gun and the titanium alloy block is adjusted to 190-210 mm, the horizontal movement speed of the spray gun is adjusted to 800 mm / s±10 mm / s, the powder feeding rate is adjusted to 5 r / min, and the second spraying is carried out; (6) After the second spraying, the horizontal movement speed of the spray gun is adjusted to 1200 mm / s±10 mm / s, and the third spraying is performed, thereby preparing an aluminum-copper-iron-boron quasi-crystal-silicon carbide coating.
3. The method for preparing the aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating according to claim 2, characterized in that: The chemical materials used in the preparation method of the aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating are: aluminum powder, iron powder, copper powder, boron powder, argon, nitrogen, silicon carbide powder, hydrogen, corundum, and the combined preparation amounts are as follows: The method for preparing the aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating comprises: 1) Prepare powder 1.1) Select 200 mesh aluminum powder, copper powder, iron powder and boron powder; 1.2) Weigh 120.7g±0.1g of aluminum powder, 123.7g±0.1g of copper powder, 53.0g±0.1g of iron powder, and 2.5g±0.1g of boron powder, and put the weighed aluminum powder, copper powder, iron powder, and boron powder into a vacuum drying oven for drying at a temperature of 200°C, a drying time of 120min, and a vacuum degree of 2Pa; 2) Aerosolization 2.1) Open the magnetic levitation vacuum melting furnace and clean the melting crucible of the vacuum melting furnace; 2.2) introducing the dried aluminum powder, copper powder, iron powder and boron powder into a smelting crucible; 2.3) The magnetic suspension vacuum melting furnace is closed and sealed, and then the air in the furnace is extracted by the vacuum pump in the vacuum melting furnace to make the pressure in the furnace reach 1Pa; 2.4) Turn on the argon device of the magnetic levitation vacuum melting furnace, input argon into the furnace and adjust the pressure in the furnace through the outlet valve of the vacuum melting furnace. The argon delivery speed is 250cm 3 / min, and keep the pressure in the furnace constant at 1Pa; 2.5) Turn on the heater of the magnetic levitation vacuum melting furnace to heat at a temperature of 950°C ± 1°C, melt the aluminum powder, copper powder, iron powder and boron powder into a melt, and when the melt temperature reaches 950°C ± 1°C, keep it warm for 3 minutes; 2.6) Start atomization, use argon gas with a purity of 99.999% to gas atomize the melt, and the atomization pressure is 2.5±0.1MPa, thereby atomizing the melt into droplets and then solidifying into powder to obtain Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder; 3) Screening and mixing powders 3.1) First use a 65μm standard mesh to filter Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasi-crystal powder, and then Al 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasicrystal powder was screened with a 45 μm standard mesh; 3.2) Sifting silicon carbide powder with a 45 μm standard mesh; 3.3) The screened Al 59 Cu 25 Fe 12.6 B 3.4 The quaternary quasicrystal powder and silicon carbide powder were mixed in a mass ratio of 1:2 and then placed in a planetary ball mill for mixing. The ball mill speed was 200 r / min and the mixing time was 10 min. 4) Prepare the base material 4.1) Cut the TC4 titanium alloy into titanium alloy blocks with a size of 50 mm × 50 mm × 10 mm using a block cutter; 4.2) Use 800-grit sandpaper to polish the surface of the titanium alloy block to make it bright; 4.3) Cleaning the surface of the titanium alloy block with acetone solution; 5) Use hypersonic flame spraying equipment for spraying 5.1) Clamp the titanium alloy block with a mold; 5.2) Adjust the distance between the spray gun of the hypersonic flame spraying equipment and the titanium alloy block to 180 mm, and keep the spray gun parallel to the titanium alloy block; 5.3) Start the air compressor of the hypersonic flame spraying equipment to backflush the spraying room to keep it clean; 5.4) Start the hypersonic flame spraying equipment and preheat the titanium alloy block 10 times; 5.5) Pour the corundum powder into the powder feeder of the hypersonic flame spraying equipment, turn on the powder feeder, and use the corundum powder in the powder feeder to sandblast the titanium alloy block, sandblasting twice; 5.6) Turn off the powder feeder, pour out the corundum powder, and pour in the mixed Al 59 Cu 25 Fe 12.6 B 3.4 Quaternary quasicrystal powder and silicon carbide powder; 5.7) Start the spray gun, set the horizontal speed of the spray gun to 1200mm / s±10mm / s, the power of the spray gun to 200kw±1kw, the pressure of the spray gun to 437.8Kpa±0.1Kpa, the oxygen-fuel ratio to 94:76, and after the sound of the spray gun becomes stable, start the powder feeder with a powder feed rate of 3r / min. When the flame of the spray gun changes from blue to red, start the first spraying; 5.8) After the first spraying, the distance between the spray gun and the titanium alloy block is adjusted to 200mm, the horizontal movement speed of the spray gun is adjusted to 800mm / s±10mm / s, the powder feeding rate is adjusted to 5r / min, and the other parameters are consistent with the parameters of the first spraying, and the second spraying is carried out; 5.9) After the second spraying, the horizontal movement speed of the spray gun is adjusted to 1200 mm / s±10 mm / s, and the other parameters are consistent with the parameters of the second spraying, and the third spraying is carried out to prepare the aluminum-copper-iron-boron quasi-crystal-silicon carbide coating. 6) Detection, analysis, and characterization The morphology of the prepared aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating was analyzed using a scanning electron microscope, and the XRD analysis of the prepared aluminum-copper-iron-boron quaternary quasi-crystal-silicon carbide coating was performed using an X-ray diffractometer.