A nondestructive detection method for steel bar corrosion in concrete under marine environment
By designing an electrochemical detection test block in a marine environment, using pre-embedded reference electrode holes and embedded graphite counter electrodes to simulate the changes in seawater tidal range, the accuracy and stability of steel bar corrosion monitoring in concrete in the marine environment were solved. Achieving long-term rapid and continuous detection results.
Patent Information
- Application Number
- CN202410498691.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-24
AI Technical Summary
The existing technology is difficult to accurately monitor the corrosion of steel bars in concrete for a long time in the marine environment, especially due to the damage to the reference electrode caused by the high-alkali and high-salt environment and the difficulty in controlling the wetting of the external counter electrode, resulting in large errors and poor repeatability of the measurement results. .
An electrochemical detection test block was designed, which used pre-embedded reference electrode holes and embedded graphite counter electrodes. It was sealed with epoxy resin and tested in simulated seawater. The step-distributed reference electrode holes and graphite electrodes were used to simulate Seawater tidal range changes to monitor chloride ion penetration rate and steel corrosion rate.
It achieves long-term rapid, continuous and accurate detection of steel corrosion in concrete, reduces measurement errors, ensures the stability and accuracy of monitoring, and avoids the error influence of external electrodes on the contact surface.
Smart Images

Figure CN118090846B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electrochemical nondestructive detection of corrosion, and in particular to a nondestructive detection method for steel bar corrosion in concrete under marine environment. Background Art
[0002] The marine environment is a complex and harsh corrosion environment. Seawater itself is a strong corrosive medium with extremely high chloride ion concentrations. Other salt substances can cause corrosion and cracking of materials. At the same time, the waves, tides, and currents of seawater produce low-frequency reciprocating stress and impact on components. In addition, marine microorganisms, attached organisms, and their metabolites directly or indirectly accelerate the corrosion process. Marine corrosion is mainly local corrosion caused by chloride ions, that is, corrosion that starts from the surface of the component and occurs in a very small area, such as galvanic corrosion, pitting corrosion, crevice corrosion, stress corrosion cracking, etc. In addition, there are low-frequency corrosion fatigue microbial corrosion, which can easily cause serious corrosion consequences.
[0003] Compared with metal components, the corrosion rate of reinforced concrete structures in marine environments is slower, but during long-term use, chloride ions continue to penetrate into the concrete and gradually corrode the deeply buried steel bars. The entire corrosion process is slow and difficult to detect. Once the reinforced concrete structure fails, it cannot be predicted or prevented, and the losses caused are particularly huge.
[0004] In actual engineering construction, the durability of reinforced concrete is an important basis for evaluating the quality of the project, and corrosion is an important factor affecting the durability of reinforced concrete. In most experiments, it is necessary to characterize corrosion by detecting electrochemical signals. The three-electrode test method, as a mature test method in the field of metal corrosion, is also applicable to the detection of steel corrosion in concrete. For the three-electrode test system, its test system contains two loops. One loop is composed of a working electrode and a reference electrode for testing the electrochemical reaction process of the working electrode. The reference electrode plays the role of accurately controlling the electrode point of the working electrode; the other loop is composed of a working electrode and a counter electrode, which plays the role of transmitting electrons to form an electrolytic cell loop. Because the three-electrode system separates the reference electrode from the counter electrode, the potential of the working electrode is not affected by the potential of the counter electrode, which can more accurately study the electrochemical reaction. However, the existing monitoring of steel corrosion in concrete under marine environment is that most of the test blocks are pre-buried reference electrodes and external counter electrodes. The high alkali and high salt environment inside the concrete will destroy the reference electrode, resulting in the inability to perform electrochemical monitoring inside the concrete for many years. At the same time, the external counter electrode needs to wet the concrete contact surface first. The wetting conditions cannot be accurately controlled each time, and the test results have large errors.
[0005] Researchers at home and abroad have designed some test methods to solve the problem of electrochemical detection difficulties in concrete under marine environment. Patent ZL 202310527258.6 discloses an electrochemical test device and method for the formation process of steel bar passivation film in concrete, in which a working electrode, an auxiliary electrode and a reference electrode are pre-buried in concrete. The patent uses a stainless steel bar with the same size as the working electrode steel bar as an auxiliary electrode. The size of the auxiliary electrode should be larger than that of the working electrode. The reason is that under the same current, if the electrode area is large, the current density is small. According to the BV equation, its overpotential is small and the polarization is small, so the electrochemical workstation has high sensitivity and low interference. However, the effective area of the auxiliary electrode in this patent is too small, and the edge electric field is unevenly distributed, resulting in inaccurate electrochemical measurement results and poor repeatability. ZL 201120099025.3 uses a dense array working electrode, which is cumbersome to operate during the sample preparation process, and requires high sample preparation accuracy. In addition, platinum electrodes are used as auxiliary electrodes, which are costly. The reference electrode is in contact with the concrete through a U-shaped tube. If the electrochemical measurement is disturbed by external factors, such as vibration, the result will fluctuate greatly. ZL 202220359578.6 provides an electrochemical test block for steel corrosion in concrete. This patent only designs the working electrode, and does not mention the auxiliary electrode and reference electrode, which will have a great impact on the electrochemical measurement results. Summary of the invention
[0006] The purpose of the present invention is to provide a testing device and method for electrochemically monitoring the destruction and corrosion process of the passive film of steel bars in concrete, which can quickly, continuously and accurately detect and analyze the penetration depth of chloride ions in concrete for a long time, and determine the destruction and corrosion time of the passive film of steel bars in concrete.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] A nondestructive detection method for steel corrosion in concrete under a marine environment, wherein an electrochemical detection test block for steel corrosion in concrete includes steel bars, wires, graphite counter electrodes, multiple pre-embedded reference electrode holes and a concrete body. The steel bars are used as working electrodes, one end of which is welded with a copper wire and pre-embedded in the concrete body. The graphite counter electrode is embedded in one side of the concrete, parallel to the steel bars. The pre-embedded reference electrode holes are made of acrylic material and are distributed in a stepped manner between the pre-embedded steel bars and the graphite counter electrode. After the concrete solidifies, five surfaces are sealed with epoxy resin, leaving a working surface for simulated seawater infiltration.
[0009] The processing process of the electrochemical test block for steel bar corrosion in concrete is as follows: the sample is prepared using a prefabricated ABS plastic sample mold. First, the mold is positioned and punched, and the acrylic reference electrode hole is fixed on the mold. The reference electrode hole extends 20mm outside the mold for electrochemical measurement. The reference electrode holes are distributed in a trapezoidal shape on the inside of the mold, and the reference electrode holes close to the steel bars are longer than the holes close to the concrete working surface.
[0010] A copper wire is welded to one end of the test steel bar and then fixed in the mold. The graphite electrode is processed into a thin sheet and inserted into one side of the mold in parallel with the reference electrode hole and the steel bar. Then concrete is poured into the ABS plastic sample mold in proportion. After 24 hours, the ABS plastic sample mold on the surface is removed and then cured in a standard curing room for 28 days.
[0011] After the concrete is cured, the five faces of the concrete block are coated with epoxy resin and cured, leaving one working surface for simulated seawater infiltration.
[0012] The experimental process of the electrochemical test block for steel corrosion in concrete is as follows: Before the electrochemical test begins, prepare a sponge or cork and immerse it in simulated seawater, and then put it into the reference electrode hole. After the reference electrode hole is completely wetted, put the reference electrode in. The reference electrode can be a copper sulfate reference electrode. The built-in wet sponge or cork is used to ensure that the reference electrode is in close contact with the surface of the concrete sample.
[0013] Afterwards, the electrochemical test block was placed in simulated seawater and tested using a classic three-electrode system, with a copper sulfate electrode as the reference electrode, a graphite plate on the concrete surface as the auxiliary electrode, and a steel bar as the working electrode. The electrochemical test began after the interior was moistened.
[0014] During the test, different ebb and flow times can be designed to simulate the changes in seawater tidal range according to the on-site conditions. When the tide is high, the test block is submerged, and the chloride ion penetration rate is faster; when the tide is low, the test block is dry, and the chloride ion penetration is stagnant. Alternating and repeating, the chloride ion penetration rate in the electrochemical measurement test block also changes with the tidal fluctuation cycle, and the corresponding corrosion rate of the steel bars in the concrete also changes accordingly. The reference electrodes at different heights measure the corresponding open circuit potential of the graphite electrode, which can characterize the seawater penetration rate of steel bar samples at different heights during different ebb and flow cycles during the tidal fluctuation process.
[0015] Furthermore, the electrochemical test block for steel bar corrosion in concrete can be designed to be rectangular or square according to the simulated test conditions, and only one side is ensured to be immersed in seawater.
[0016] Furthermore, the distance between the steel bar and the graphite counter electrode is 20-80 mm.
[0017] Furthermore, each reference electrode hole has an inner diameter of 2-10 mm so that the reference electrode can be inserted during measurement, and the reference electrode holes are spaced 5-20 mm apart and are distributed in a stepped manner inside the concrete protective layer. The height difference between the reference electrodes is 3-10 mm.
[0018] Furthermore, the reference electrode hole is moistened with a sponge or cork before use and maintained in a moist state to form a loop with the steel bar to be tested and the graphite electrode, which can be used to monitor electrochemical signals such as the penetration depth of chloride ions in concrete, the impedance of reinforced concrete, and the half-cell potential.
[0019] Furthermore, the tidal range changes can be added to the simulated seawater to measure the penetration process of seawater into concrete and the corrosion rate of steel bars in different tidal range cycles.
[0020] Advantages of the present invention:
[0021] The electrochemical test block has a simple structure and a simple preparation method. The molding mold is a plastic mold, which is easy to dismantle. The method of pre-embedded reference electrode is abandoned, and a pre-embedded reference electrode hole is adopted. One hole can be used for multiple purposes, and different reference electrodes can be used to monitor a variety of electrochemical signals. At the same time, since the reference electrode can be disassembled after the test, it will not cause damage to the reference electrode, and long-term monitoring of concrete can be truly realized. The embedded graphite counter electrode is used, and the contact between the electrode and the concrete is stable, avoiding measurement errors caused by factors such as wetting and loose contact between the external counter electrode and the concrete. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments:
[0023] Figure 1 Schematic diagram of the electrochemical test block for steel corrosion in concrete;
[0024] Figure 1 In the figure, 1 is an electrochemical workstation, 2 is epoxy resin, 3 is a reference reserved hole, 4 is concrete, 5 is a steel bar, and 6 is a graphite electrode. DETAILED DESCRIPTION
[0025] Example 1
[0026] A nondestructive detection method for steel corrosion in concrete under a marine environment, wherein an electrochemical detection test block for steel corrosion in concrete includes steel bars, wires, graphite counter electrodes, multiple pre-embedded reference electrode holes and a concrete body. The steel bars are used as working electrodes, one end of which is welded with a copper wire and pre-embedded in the concrete body. The graphite counter electrode is embedded in one side of the concrete, parallel to the steel bars. The pre-embedded reference electrode holes are made of acrylic material and are distributed in a stepped manner between the pre-embedded steel bars and the graphite counter electrode. After the concrete solidifies, five surfaces are sealed with epoxy resin, leaving a working surface for simulated seawater infiltration.
[0027] Electrochemical test specimens for steel corrosion in concrete, see Figure 1 The processing process is as follows: the sample is prepared using a prefabricated ABS plastic sample mold. First, the mold is positioned and punched, and the acrylic reference electrode hole is fixed on the mold. The reference electrode hole extends 20mm outside the mold for electrochemical measurement. The reference electrode holes on the inside of the mold are distributed in a trapezoidal shape, and the reference electrode holes close to the steel bars are longer than those close to the concrete working surface.
[0028] A copper wire is welded to one end of the test steel bar and then fixed in the mold. The graphite electrode is processed into a thin sheet and inserted into one side of the mold in parallel with the reference electrode hole and the steel bar. Then concrete is poured into the ABS plastic sample mold in proportion. After 24 hours, the ABS plastic sample mold on the surface is removed and then cured in a standard curing room for 28 days.
[0029] After the concrete is cured, the five faces of the concrete block are coated with epoxy resin and cured, leaving one working surface for simulated seawater infiltration.
[0030] The experimental process of the electrochemical test block for steel corrosion in concrete is as follows: Before the electrochemical test begins, prepare a sponge or cork and immerse it in simulated seawater, and then put it into the reference electrode hole. After the reference electrode hole is completely wetted, put the reference electrode in. The reference electrode can be a copper sulfate reference electrode. The built-in wet sponge or cork is used to ensure that the reference electrode is in close contact with the surface of the concrete sample.
[0031] Afterwards, the electrochemical test block was placed in simulated seawater and tested using a classic three-electrode system, with a copper sulfate electrode as the reference electrode, a graphite plate on the concrete surface as the auxiliary electrode, and a steel bar as the working electrode. The electrochemical test began after the interior was moistened.
[0032] During the test, different ebb and flow times can be designed to simulate the changes in seawater tidal range according to the on-site conditions. When the tide is high, the test block is submerged, and the chloride ion penetration rate is faster; when the tide is low, the test block is dry, and the chloride ion penetration is stagnant. Alternating and repeating, the chloride ion penetration rate in the electrochemical measurement test block also changes with the tidal fluctuation cycle, and the corresponding corrosion rate of the steel bars in the concrete also changes accordingly. The reference electrodes at different heights measure the corresponding open circuit potential of the graphite electrode, which can characterize the seawater penetration rate of steel bar samples at different heights during different ebb and flow cycles during the tidal fluctuation process.
[0033] Furthermore, the electrochemical test block for steel bar corrosion in concrete can be designed to be rectangular or square according to the simulated test conditions, and only one side is ensured to be immersed in seawater.
[0034] Furthermore, the distance between the steel bar and the graphite counter electrode is 20-80 mm.
[0035] Furthermore, each reference electrode hole has an inner diameter of 2-10 mm so that the reference electrode can be inserted during measurement, and the reference electrode holes are spaced 5-20 mm apart and are distributed in a stepped manner inside the concrete protective layer. The height difference between the reference electrodes is 3-10 mm.
[0036] Furthermore, the reference electrode hole is moistened with a sponge or cork before use and maintained in a moist state to form a loop with the steel bar to be tested and the graphite electrode, which can be used to monitor electrochemical signals such as the penetration depth of chloride ions in concrete, the impedance of reinforced concrete, and the half-cell potential.
[0037] Furthermore, the tidal range changes can be added to the simulated seawater to measure the penetration process of seawater into concrete and the corrosion rate of steel bars in different tidal range cycles.
[0038] Sample preparation:
[0039] (1) Sample preparation: Use an ABS plastic sample mold of 150mm×150mm×150mm. First, position and punch holes on the mold, and fix four acrylic reference electrode holes with an inner diameter of 8mm on the mold to facilitate electrochemical measurement. The reference electrode holes are distributed in a trapezoidal shape on the inside of the mold, with a spacing of 10mm between the reference electrode holes, and are distributed in a stepped manner inside the concrete protective layer. The height difference between the reference electrodes is 5mm, and the reference electrode holes close to the steel bars are 5mm longer than the holes close to the concrete working surface.
[0040] (2) Weld a copper wire to one end of a φ10mm×120mm steel bar and fix it in the mold. Process a graphite electrode into 150mm×150mm×5mm and insert it into one side of the mold parallel to the reference electrode hole and the steel bar. Then pour concrete in proportion.
[0041] (3) Remove the mold after 24 hours and then cure in a standard curing room for 28 days.
[0042] Test method:
[0043] After the concrete specimens were cured for 28 days, the concrete was immersed in a simulated seawater solution, and the electrochemical test was started after the inside was moistened. The test was carried out using a classic three-electrode system, that is, the copper sulfate electrode was used as the reference electrode, the graphite plate on the concrete surface was used as the auxiliary electrode, and the steel bar was used as the working electrode. The electrochemical experiments were all carried out on a Gamry electrochemical workstation. During the electrochemical test, the concrete sample was immersed in tap water, and a wet sponge was built into the reference electrode hole to ensure that the reference electrode was in close contact with the surface of the concrete sample. After the electrochemical system was stable, the linear polarization resistance test polarized the steel bar sample from -10 mV to +10 mV relative corrosion potential, with a scan rate of 0.17 mV / s. The ohmic drop between the working electrode and the reference electrode can be automatically compensated by the instrument. This test can obtain two electrochemical parameter values: corrosion potential and polarization resistance. The EIS test scan frequency ranged from 100 kHz to 10 mHz, and all tests were carried out at open circuit potential with an applied AC voltage of 10 mV.
[0044] Two test methods are used to simulate seawater. One is static immersion to test the rate of seawater penetration into concrete and the corrosion rate of steel bars under static conditions, and to compare the effects of different reference electrode positions on electrochemical measurement results. The other is a tidal range experiment, that is, seawater undergoes periodic ebb and flow. The ebb and flow time is 6 hours, and a complete ebb and flow process is completed within 12 hours. The concrete electrochemical specimen is placed at the highest tide level.
[0045] Matters not covered by the present invention are known technologies.
[0046] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. A nondestructive detection method for steel bar corrosion in concrete under marine environment, characterized by: The nondestructive detection method for steel corrosion in concrete under marine environment, the test block includes steel bars, wires, graphite counter electrodes, multiple pre-embedded reference electrode holes and concrete body; wherein the steel bars are used as working electrodes, one end of which is welded with a copper wire and pre-embedded in the concrete body, the graphite counter electrode is embedded in one side of the concrete, parallel to the steel bars, the pre-embedded reference electrode holes are made of acrylic material, and are distributed in a stepped manner between the pre-embedded steel bars and the graphite counter electrode; after the concrete solidifies, five surfaces are sealed with epoxy resin, leaving a working surface for simulated seawater infiltration; The processing process of the electrochemical test block for steel bar corrosion in concrete is as follows: the sample is prepared using a prefabricated ABS plastic sample mold, firstly, a hole is positioned and punched on the mold, and an acrylic reference electrode hole is fixed on the mold, and the reference electrode hole extends 20 mm outside the mold for electrochemical measurement; the reference electrode holes on the inside of the mold are distributed in a trapezoidal shape, and the reference electrode holes close to the steel bars are longer than the holes close to the concrete working surface; A copper wire is welded to one end of the test steel bar and then fixed in the mold. A graphite counter electrode is processed into a thin sheet and inserted into one side of the mold in parallel with the reference electrode hole and the steel bar. Then concrete is poured into the ABS plastic sample mold in proportion. After 24 hours, the ABS plastic sample mold on the surface is removed and then cured in a standard curing room for 28 days. After the concrete curing is completed, the five faces of the concrete block are coated with epoxy resin and cured, leaving one working face for simulated seawater infiltration; The experimental process of the electrochemical test block for steel bar corrosion in concrete is as follows: before the electrochemical test begins, a sponge or cork is prepared in advance and immersed in simulated seawater, and then placed in the reference electrode hole; after the reference electrode hole is completely wetted, a reference electrode is placed, and a copper sulfate reference electrode is selected as the reference electrode. The built-in wet sponge or cork is used to ensure that the reference electrode is in close contact with the surface of the concrete sample; Afterwards, the electrochemical test block was placed in simulated seawater for testing, using a copper sulfate electrode as a reference electrode, a graphite counter electrode on the concrete surface as an auxiliary electrode, and a steel bar as a working electrode; the electrochemical test was started after the interior was moistened.
2. The method for nondestructive detection of steel bar corrosion in concrete under marine environment according to claim 1, characterized in that: The designed and processed electrochemical test block for steel bar corrosion in concrete can be designed into a rectangular or square shape according to the simulated test conditions, and only one side is ensured to be immersed in seawater.
3. The method for nondestructive detection of steel bar corrosion in concrete under marine environment according to claim 1, characterized in that: The distance between the steel bar and the graphite counter electrode is 20-80 mm.
4. The method for nondestructive detection of steel bar corrosion in concrete under marine environment according to claim 1, characterized in that: The inner diameter of the reference electrode hole is 2-10 mm, so that the reference electrode can be inserted during measurement, and the reference electrode hole spacing is 5-20 mm, distributed in a stepped manner inside the concrete protective layer; the height difference between the reference electrodes is 3-10 mm.
5. The method for nondestructive detection of steel bar corrosion in concrete under marine environment according to claim 1, characterized in that: The reference electrode hole is moistened with a sponge or a cork before use and kept moistened to form a loop with the steel bar and the graphite counter electrode to monitor the electrochemical signals of the chloride ion penetration depth in the concrete, the steel bar concrete impedance and the half-cell potential.
Citation Information
Patent Citations
Electrochemical testing device and method for generation process of steel bar passivation film in concrete
CN116754621A
Laboratory detection test cube simulating reinforced concrete electrochemical corrosion
CN202110125U
Electrochemical detection test block for steel bar corrosion in concrete
CN217112001U
Real-time monitoring sensor for durability of concrete structures and fabricating method thereof
CN102680387A
Corrosion detecting probes for use with a corrosion-rate meter for electrochemically determining the corrosion rate of reinforced concrete structures
US5259944A