A low-temperature metal bonding preparation method for high-performance samarium-iron-nitrogen composite magnet

Through the preparation method of low-temperature metal bonding, tin or tin alloy and ferrite powder, the decomposition and cost problems caused by high-temperature sintering of samarium-ferro-nitrogen magnets are solved, and high-performance and high-density samarium-ferro-nitrogen composite magnets are achieved. Preparation, suitable for large-scale production and improves antioxidant capacity.

CN118098808BActive Publication Date: 2024-11-26ANHUI UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410421510.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-09
Publication Date
2024-11-26
Estimated Expiration
2044-04-09

AI Technical Summary

Technical Problem

The existing preparation methods for samarium-ferro-nitrogen magnets have problems such as high-temperature sintering, resulting in material decomposition, high cost and low magnet density, making it difficult to achieve high performance and large-scale mass production.

Method used

The preparation method of low-temperature metal bonding is adopted, using tin or tin alloy as the adhesive, combined with ferrite powder, and hot press orientation and nitrogen oven curing are carried out at low temperatures to reduce the amount of adhesive, and improve magnet density and anti-oxidation properties.

Benefits of technology

Preparing high-performance samarium-iron-nitrogen composite magnets at lower temperatures reduces the requirements of powder passivation treatment, reduces environmental pollution, improves the magnetic properties and oxidation resistance of magnets, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118098808B_ABST
    Figure CN118098808B_ABST
Patent Text Reader

Abstract

The present invention provides a low-temperature metal bonding preparation method for a high-performance samarium iron nitrogen composite magnet, and relates to the technical field of magnetic material preparation. The high-performance samarium iron nitrogen composite magnet is prepared by using a passivation solution and ethanol to perform antioxidant modification on crushed magnetic powder, and then adding ferrite powder, and using tin / tin alloy powder as an adhesive to prepare a bonded magnet at a relatively low temperature. The present invention overcomes the shortcomings of the prior art, can improve the density of the composite magnet while reducing the amount of the adhesive, and comprehensively improves the magnetic properties of the magnet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of magnetic material preparation, and in particular to a low-temperature metal bonding preparation method for a high-performance samarium-iron-nitrogen composite magnet. Background Art

[0002] In recent years, due to the continuous development of new energy vehicles, wind turbines, white appliances and other industries, rare earth permanent magnet materials represented by NdFeB and SmCo have been widely used due to their excellent magnetic properties and working stability. The motor industry, with the upgrading of technology, has put forward higher requirements on the performance of magnetic energy components.

[0003] Since the advent of rare earth permanent magnet materials, their production and preparation technologies have been rapidly iterating, and they can be divided into sintered permanent magnet materials and bonded permanent magnet materials due to different processes and characteristics. Bonded permanent magnet materials can be divided into molded bonded permanent magnet materials (generally resin is used as a binder), injection bonded permanent magnet materials (the binder is mainly nylon, polyoxymethylene and other thermoplastics as a binder) and calendered bonded permanent magnet materials (the binder is generally modified rubber). Since bonded magnetic materials are complexed by organic media, there is no high-temperature sintering step in the process flow, which can effectively avoid material deformation caused by high-temperature sintering. It has the advantages of high dimensional accuracy, can be molded in one step, and is easy to mass-produce. Bonded magnetic materials have also been widely used in emerging technology industries due to their extremely strong shaping ability.

[0004] Recently, high-temperature sintering samarium iron nitrogen technology represented by the sps method (spark plasma sintering technology) has begun to appear, which has the characteristics of high density of prepared magnets and good product consistency. The public patent CN116052972A mentions a method for preparing samarium iron nitrogen magnets using the sps method, and produces high-performance, high-density samarium iron nitrogen magnets, but the cost of preparing samarium iron nitrogen magnets by spark plasma sintering is high, and it is difficult to mass produce on a large scale, and the high-temperature sintering process will cause the decomposition of samarium iron nitrogen and reduce the magnetic properties; Patent No. CN105225780B mentions a method for producing samarium iron nitrogen bonded magnets using sodium silicate as the main adhesive. This method can achieve bonding at a relatively low temperature and avoid the problem of samarium iron nitrogen decomposition caused by high-temperature sintering. It has the potential for large-scale mass production. However, in this bonding process, there are disadvantages of using a high content of adhesive and low density of the product magnet. In addition, the preparation of bonded magnets with a single samarium iron nitrogen magnetic powder also has the disadvantage of low density. Therefore, it is necessary to optimize the preparation method of the magnet to comprehensively improve its performance. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a low-temperature metal bonding preparation method for a high-performance samarium-iron-nitrogen composite magnet, which can increase the density of the composite magnet while reducing the amount of binder used, and comprehensively improve the magnetic properties of the magnet.

[0006] To achieve the above objectives, the technical solution of the present invention is implemented through the following technical solutions:

[0007] A low-temperature metal bonding preparation method for a high-performance samarium-iron-nitrogen composite magnet, the preparation process comprising the following steps:

[0008] S1. Preparation of Sm2Fe 17 The alloy is spun off the belt, crushed and ground to prepare samarium iron alloy fine powder, and then the samarium iron alloy fine powder is nitrided to obtain Sm2Fe 17 N3 magnetic powder, later Sm2Fe 17 N3 magnetic powder is put into a ball mill and mixed with a surfactant for wet grinding to obtain magnetic powder for use;

[0009] S2, uniformly mixing the magnetic powder and anhydrous ethanol in a passivation tank to prepare a mixed slurry, and then adding a mixed passivation solution to the mixed slurry for heating and passivation until the ethanol is completely evaporated to obtain a modified samarium iron nitrogen magnetic powder with antioxidant properties;

[0010] S3. Put the modified SmFeN magnetic powder, ferrite powder and tin / tin alloy powder into a mixing tank and mix them evenly to prepare a mixed powder. Then fill the mixed powder into a hot pressing mold and orient it under low temperature hot pressing at 220℃-240℃. After the hot pressing, put the magnet into a nitrogen oven and heat it to 160℃-220℃ for curing. After the curing, a low temperature sintered composite SmFeN magnet is obtained.

[0011] Preferably, the specific method of crushing and grinding to prepare the samarium-iron alloy fine powder in step S1 is to firstly hydrogen-crush the alloy strip, and then use a jet mill to crush the alloy strip at high speed using nitrogen to obtain the samarium-iron alloy fine powder.

[0012] Preferably, the samarium-iron alloy fine powder is nitrided in step S1 by transferring the samarium-iron alloy fine powder into a hydrogen cracking furnace, replacing the nitrogen source, and heating it to 450° C.-500° C. and keeping it for 720 min-960 min to fully nitridize.

[0013] Preferably, the wet grinding method in step S1 is to select anhydrous ethanol or heptane as the wet grinding medium, and the amount of surfactant added to the magnetic powder is 0.1wt%-2.0wt%, the ball-to-material ratio is 20:1-40:1, the ball milling is 9h-15h, and any one of glucol, oleic acid, and pvp (polyvinyl pyrrolidone) is selected as the surfactant.

[0014] Preferably, the amount of anhydrous ethanol added to the mixed slurry in step S2 is 5wt% to 10wt%.

[0015] Preferably, the mixed passivation solution in step S2 is phosphoric acid and a silane coupling agent, and the amount of phosphoric acid added to the modified samarium iron nitrogen magnet is 0.2wt%-2wt%, and the amount of silane coupling agent added is 0wt%-1.2wt%.

[0016] Preferably, in the mixed powder of step S3, the amount of ferrite powder added is 1wt% to 10wt%, the amount of tin / tin alloy powder added is 1wt% to 5wt%, and the rest is modified samarium iron nitrogen magnetic powder.

[0017] Preferably, the ferrite powder in step S3 is one or a mixture of strontium ferrite powder and barium ferrite powder, and the average particle size of the ferrite powder is 1 μm-3 μm.

[0018] Preferably, the particle size of the tin / tin alloy powder in step S3 is 25 μm-80 μm.

[0019] Preferably, the pressure of the hot pressing orientation in step S3 is 25 MPa-38 MPa, the holding time is 30 s-120 s, and the magnet is heated and kept warm in the nitrogen oven for 30 min-60 min.

[0020] The present invention provides a low-temperature metal bonding preparation method for a high-performance samarium-iron-nitrogen composite magnet, which has the following advantages over the prior art:

[0021] (1) The present invention uses low-temperature metals such as tin or tin alloy as adhesives, which reduces the amount of adhesive used and improves the density of the composite magnet. The bonded magnet can be prepared at a relatively low temperature (200°C), which is lower than the decomposition temperature of samarium iron nitrogen magnetic powder (500°C-620°C), thereby improving the product yield and reducing the requirements for powder passivation treatment, thereby reducing environmental pollution.

[0022] (2) The composite samarium iron nitrogen magnet with ferrite added in the present invention improves the magnet performance, and the magnet has obvious anti-oxidation ability, and still has obvious anti-oxidation ability in an air environment of 100°C-200°C; BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The X-ray diffraction pattern of the large-particle samarium iron nitrogen magnetic powder prepared in step (1) of Example 1 of the present invention;

[0024] Figure 2 This is a scanning electron microscope photograph of the large-particle samarium iron nitrogen magnetic powder prepared in step (1) of Example 1 of the present invention;

[0025] Figure 3 The X-ray diffraction pattern of the samarium iron nitrogen magnet powder prepared in step (3) of Example 1 of the present invention;

[0026] Figure 4MH curve of the modified samarium iron nitrogen magnetic powder prepared in Example 1 of the present invention;

[0027] Figure 5 MH curve of the modified samarium iron nitrogen magnetic powder prepared in Example 4 of the present invention;

[0028] Figure 6 This is the MH curve of the modified samarium iron nitrogen magnetic powder prepared in Example 5 of the present invention.

[0029] Figure 7 This is the MH curve of the oxidation resistance test (100°C / 5min) of the modified SmFeN magnetic powder prepared in Example 5 of the present invention.

[0030] Figure 8 This is the MH curve of the oxidation resistance test (200°C / 5min) of the modified SmFeN magnetic powder prepared in Example 5 of the present invention. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Embodiment 1:

[0033] Preparation of SmFeN composite magnets:

[0034] (1) 25wt% samarium ingot and 75wt% iron ingot were put into a rapid solidification belt furnace and the crucible temperature was maintained at 1450℃ to prepare Sm2Fe 17 Throwing belt piece;

[0035] The strip was placed in a hydrogen cracking furnace and heated to 550°C for 6 hours to obtain a coarse powder of samarium-iron alloy;

[0036] The coarse powder is put into the air flow mill, and the sieve cage speed is set to 3000 rpm to obtain finer samarium iron alloy powder;

[0037] The fine alloy powder is placed in a hydrogen cracking furnace with nitrogen gas source, heated to 475℃ and kept warm for 720min to obtain fully nitrided large-particle samarium iron nitrogen magnetic powder;

[0038] The samarium iron nitrogen powder was put into a ball mill with a ball-to-material ratio of 20:1, 1 wt% of glucitol was added, alcohol was used as a wet grinding medium, the speed was set to 180 rpm, and the ball milling was performed for 18 hours to obtain small-size samarium iron nitrogen magnetic powder;

[0039] (2) mixing small-size samarium iron nitrogen magnetic powder with 1 wt % phosphoric acid and 5 wt % ethanol in a passivation tank and heating the mixture until the ethanol is completely evaporated to obtain modified samarium iron nitrogen powder;

[0040] (3) The modified SmFeN powder and 1 wt% tin powder (300 mesh) were placed in a mixing tank and mixed at 30 rpm for 10 min. The mixed powder was placed in a composite hot press, the temperature was raised to 230°C, a 2T oriented magnetic field was applied, and the pressure was maintained at 30 MPa for 60 s to obtain a standard column with a diameter of 15 mm. The standard column was placed in a nitrogen-protected oven and the temperature was set to 160°C for 60 min to obtain a finished SmFeN magnet.

[0041] Embodiment 2:

[0042] Preparation of SmFeN composite magnets:

[0043] (1) 25wt% samarium ingot and 75wt% iron ingot were put into a rapid solidification belt furnace and the crucible temperature was maintained at 1450℃ to prepare Sm2Fe 17 Throwing belt piece;

[0044] The strip was placed in a hydrogen cracking furnace and heated to 550°C for 6 hours to obtain a coarse powder of samarium-iron alloy;

[0045] The coarse powder is put into the air flow mill, and the sieve cage speed is set to 3000 rpm to obtain finer samarium iron alloy powder;

[0046] The fine alloy powder is placed in a hydrogen cracking furnace with nitrogen gas source, heated to 475℃ and kept warm for 720min to obtain fully nitrided large-particle samarium iron nitrogen magnetic powder;

[0047] The samarium iron nitrogen powder was put into a ball mill with a ball-to-material ratio of 20:1, 1 wt% of glucitol was added, alcohol was used as a wet grinding medium, the speed was set to 180 rpm, and the ball milling was performed for 18 hours to obtain small-size samarium iron nitrogen magnetic powder;

[0048] (2) mixing small-size samarium iron nitrogen magnetic powder with 1 wt % phosphoric acid and 5 wt % ethanol in a passivation tank and heating the mixture until the ethanol is completely evaporated to obtain modified samarium iron nitrogen powder;

[0049] (3) The modified SmFeN powder, 5 wt% SrFeO powder (average particle size 2 μm) and 1 wt% Sn powder (300 mesh) were placed in a mixing tank and mixed at 30 rpm for 10 min. The mixed powder was placed in a composite hot press, the temperature was raised to 230°C, a 2T oriented magnetic field was applied, and the pressure was maintained at 30 MPa for 60 s to obtain a standard column with a diameter of 15 mm. The standard column was placed in a nitrogen-protected oven and kept at 160°C for 60 min to obtain a finished SmFeN magnet.

[0050] Embodiment 3:

[0051] Preparation of SmFeN composite magnets:

[0052] (1) 25wt% samarium ingot and 75wt% iron ingot were put into a rapid solidification belt furnace and the crucible temperature was maintained at 1450℃ to prepare Sm2Fe 17 Throwing belt piece;

[0053] The strip was placed in a hydrogen cracking furnace and heated to 550°C for 6 hours to obtain a coarse powder of samarium-iron alloy;

[0054] The coarse powder is put into the air flow mill, and the sieve cage speed is set to 3000 rpm to obtain finer samarium iron alloy powder;

[0055] The fine alloy powder is placed in a hydrogen cracking furnace with nitrogen gas source, heated to 475℃ and kept warm for 720min to obtain fully nitrided large-particle samarium iron nitrogen magnetic powder;

[0056] The samarium iron nitrogen powder was put into a ball mill with a ball-to-material ratio of 20:1, 1 wt% of glucitol was added, alcohol was used as a wet grinding medium, the speed was set to 180 rpm, and the ball milling was performed for 18 hours to obtain small-size samarium iron nitrogen magnetic powder;

[0057] (2) mixing small-size samarium iron nitrogen magnetic powder with 1 wt % phosphoric acid and 5 wt % ethanol in a passivation tank and heating the mixture until the ethanol is completely evaporated to obtain modified samarium iron nitrogen powder;

[0058] (3) The modified SmFeN powder, 10 wt% SrFe2O3 powder (average particle size 2 μm) and 1 wt% Sn powder (300 mesh) were placed in a mixing tank and mixed at 30 rpm for 10 min. The mixed powder was placed in a composite hot press, heated to 230°C, and a 2T oriented magnetic field was applied. The pressure was maintained at 30 MPa for 60 s to obtain a standard column with a diameter of 15 mm. The standard column was placed in a nitrogen-protected oven and kept at 160°C for 60 min to obtain a finished SmFeN magnet.

[0059] Embodiment 4:

[0060] Preparation of SmFeN composite magnets:

[0061] (1) 25wt% samarium ingot and 75wt% iron ingot were put into a rapid solidification belt furnace and the crucible temperature was maintained at 1450℃ to prepare Sm2Fe 17 Throwing belt piece;

[0062] The strip was placed in a hydrogen cracking furnace and heated to 550°C for 6 hours to obtain a coarse powder of samarium-iron alloy;

[0063] The coarse powder is put into the air flow mill, and the sieve cage speed is set to 3000 rpm to obtain finer samarium iron alloy powder;

[0064] The fine alloy powder is placed in a hydrogen cracking furnace with nitrogen gas source, heated to 475℃ and kept warm for 720min to obtain fully nitrided large-particle samarium iron nitrogen magnetic powder;

[0065] The SmFeN powder was put into a ball mill with a ball-to-material ratio of 20:1, 0.7 wt% PVP was added, alcohol was used as a wet grinding medium, the speed was set to 180 rpm, and the ball milling was performed for 18 hours to obtain small-size SmFeN magnetic powder;

[0066] (2) mixing small-size samarium iron nitrogen magnetic powder with 1 wt % phosphoric acid and 5 wt % ethanol in a passivation tank and heating the mixture until the ethanol is completely evaporated to obtain modified samarium iron nitrogen powder;

[0067] (3) The modified SmFeN powder and 2 wt% tin powder (300 mesh) were placed in a mixing tank and mixed at 30 rpm for 10 min. The mixed powder was placed in a composite hot press, the temperature was raised to 230°C, a 2T oriented magnetic field was applied, and the pressure was maintained at 30 MPa for 60 s to obtain a standard column with a diameter of 15 mm. The standard column was placed in a nitrogen-protected oven and kept at 160°C for 60 min to obtain a finished SmFeN magnet.

[0068] Embodiment 5:

[0069] Preparation of SmFeN composite magnets:

[0070] (1) 25wt% samarium ingot and 75wt% iron ingot were put into a rapid solidification belt furnace and the crucible temperature was maintained at 1450℃ to prepare Sm2Fe 17 Throwing belt piece;

[0071] The strip was placed in a hydrogen cracking furnace and heated to 550°C for 6 hours to obtain a coarse powder of samarium-iron alloy;

[0072] The coarse powder is put into the air flow mill, and the sieve cage speed is set to 3000 rpm to obtain finer samarium iron alloy powder;

[0073] The fine alloy powder is placed in a hydrogen cracking furnace with nitrogen gas source, heated to 475℃ and kept warm for 720min to obtain fully nitrided large-particle samarium iron nitrogen magnetic powder;

[0074] The samarium iron nitrogen powder was put into a ball mill with a ball-to-material ratio of 20:1, 2 wt% of glucitol was added, alcohol was used as a wet grinding medium, the speed was set to 180 rpm, and the ball milling was performed for 18 hours to obtain small-size samarium iron nitrogen magnetic powder;

[0075] (2) mixing small-size samarium iron nitrogen magnetic powder with 1 wt % phosphoric acid and 5 wt % ethanol in a passivation tank and heating the mixture until the ethanol is completely evaporated to obtain modified samarium iron nitrogen powder;

[0076] (3) The modified SmFeN powder and 5 wt% tin powder (300 mesh) were placed in a mixing tank and mixed at 30 rpm for 10 min. The mixed powder was placed in a composite hot press, the temperature was raised to 230°C, a 2T oriented magnetic field was applied, and the pressure was maintained at 30 MPa for 60 s to obtain a standard column with a diameter of 15 mm. The standard column was placed in a nitrogen-protected oven and kept at 160°C for 60 min to obtain a finished SmFeN magnet.

[0077] Detection:

[0078] 1. The magnetic properties of the finished samarium iron nitrogen magnets prepared in the above embodiments 1-5 were tested using a permanent magnet measuring instrument. The specific results are shown in Table 1 below:

[0079] Table 1

[0080] Group <![CDATA[B r ]]> <![CDATA[H cj ]]> <![CDATA[(BH) max ]]> Example 1 6725.10GS 12.502kOe 11.812MGsOe Example 2 7252.43GS 11.940kOe 12.425MGsOe Example 3 6570.44GS 11.156kOe 11.860MGsOe Example 4 6244.06GS 13.927kOe 11.251MGsOe Example 5 5130.95GS 9.144kOe 9.692MGsOe

[0081] In summary, the addition of tin powder and a small amount of ferrite can effectively ensure the magnetic properties of the material.

[0082] 2. X-ray diffraction test was performed on the large particle SmFeN magnetic powder, SrFeO powder and SmFeN magnet powder prepared in Example 1. The specific results are as follows: Figure 1 and Figure 3 As shown;

[0083] 3. The magnetic properties of the modified samarium iron nitrogen magnetic powders in Example 1, Example 4 and Example 5 were tested (e.g. Figure 4-5 As shown), the anti-oxidation test of the modified samarium iron nitrogen magnetic powder in Example 5 was carried out at 100°C / 5min and 200°C / 5min, and then the magnetic properties were tested again (as shown Figure 7-8 ), as shown in Table 2 below:

[0084] Table 2

[0085] Group <![CDATA[M r (emu / g)]]> <![CDATA[H cj (You)]]> Embodiment 1, 91.8 12559.5 Example 4 72.0 13666.1 Example 5 63.6 10599.6 Example 5 (100°C / 5min) 62.8 10396.7 Example 5 (100°C / 5min) 64.6 9758.3

[0086] In summary, the samarium iron nitrogen magnetic powder modified and prepared in the present application has good antioxidant effect.

[0087] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A low-temperature metal bonding preparation method for high-performance samarium iron nitrogen composite magnets, characterized in that: The preparation process comprises the following steps: S1. Preparation of Sm2Fe 17 The alloy is spun off the belt, crushed and ground to prepare samarium iron alloy fine powder, and then the samarium iron alloy fine powder is nitrided to obtain Sm2Fe 17 N3 magnetic powder, later Sm2Fe 17 N3 magnetic powder is put into a ball mill and mixed with a surfactant for wet grinding to obtain magnetic powder for use; S2, uniformly mixing the magnetic powder and anhydrous ethanol in a passivation tank to prepare a mixed slurry, and then adding a mixed passivation liquid into the mixed slurry for heat passivation until the ethanol is completely evaporated to obtain a modified samarium iron nitrogen magnetic powder with antioxidant properties, wherein the mixed passivation liquid is phosphoric acid and a silane coupling agent, and the amount of phosphoric acid added in the modified samarium iron nitrogen magnetic powder is 0.2wt%-2wt%, and the amount of silane coupling agent added is 0wt%-1.2wt%; S3. Put the modified SmFeN magnetic powder, ferrite powder and tin / tin alloy powder into a mixing tank and mix them evenly to prepare a mixed powder. Then fill the mixed powder into a hot pressing mold and orient it under low temperature hot pressing at 220℃-240℃. After the hot pressing, put the magnet into a nitrogen oven and heat it to 160℃-220℃ for curing. After the curing, a low temperature sintered composite SmFeN magnet is obtained.

2. The low-temperature metal bonding preparation method of a high-performance samarium-iron-nitrogen composite magnet according to claim 1, characterized in that: The specific method of crushing and grinding to prepare the samarium-iron alloy fine powder in step S1 is to firstly hydrogen-crush the alloy strip, and then use a jet mill to crush the alloy strip at high speed using nitrogen to obtain the samarium-iron alloy fine powder.

3. The low-temperature metal bonding preparation method of a high-performance samarium-iron-nitrogen composite magnet according to claim 1, characterized in that: The method of nitriding the samarium-iron alloy fine powder in step S1 is to transfer the samarium-iron alloy fine powder into a hydrogen cracking furnace, replace the nitrogen source, and heat it to 450° C.-500° C. and keep it for 720 min-960 min to fully nitridize.

4. The low-temperature metal bonding preparation method of a high-performance samarium-iron-nitrogen composite magnet according to claim 1, characterized in that: The wet grinding method in step S1 is to use anhydrous ethanol or heptane as the wet grinding medium, and the amount of surfactant added to the magnetic powder is 0.1wt%-2.0wt%, the ball-to-material ratio is 20:1-40:1, the ball milling is 9h-15h, and any one of glucol, oleic acid, and PVP is selected as the surfactant.

5. The low temperature metal bonding preparation method of a high performance samarium iron nitrogen composite magnet according to claim 1, characterized in that: The amount of anhydrous ethanol added to the mixed slurry in step S2 is 5wt%-10wt%.

6. The low temperature metal bonding preparation method of a high performance samarium iron nitrogen composite magnet according to claim 1, characterized in that: In the mixed powder of step S3, the added amount of ferrite powder is 1wt%~10wt%, the added amount of tin / tin alloy powder is 1wt%~5wt%, and the rest is modified samarium iron nitrogen magnetic powder.

7. The low temperature metal bonding preparation method of a high performance samarium iron nitrogen composite magnet according to claim 1, characterized in that: In the step S3, the ferrite powder is one of strontium ferrite powder and barium ferrite powder or a mixture of the two, and the average particle size of the ferrite powder is 1 μm-3 μm.

8. The low temperature metal bonding preparation method of a high performance samarium iron nitrogen composite magnet according to claim 1, characterized in that: The particle size of the tin / tin alloy powder in step S3 is 25 μm-80 μm.

9. The low temperature metal bonding preparation method of a high performance samarium iron nitrogen composite magnet according to claim 1, characterized in that: The pressure of the hot pressing orientation in step S3 is 25Mpa-38Mpa, the holding time is 30s-120s, and the magnet is heated and kept warm in the nitrogen oven for 30min-60min.