A nano-supported gold-iridium catalyst and its preparation method and application

Through the preparation of nano-supported gold-iridium catalysts, the synergistic effect of gold and iridium is used to solve the problems of insufficient catalytic activity and high cost in the existing technology, and achieve efficient and stable production of methyl methacrylate. The conversion rate and selectivity of acrolein reach 99%.

CN118122325BActive Publication Date: 2024-10-22SHANDONG SUNWAY PETROCHEMICAL ENGINEERING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410340231.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-22
Publication Date
2024-10-22
Estimated Expiration
2044-03-22

AI Technical Summary

Technical Problem

In the existing technology, gold-based catalysts used for the production of methyl methacrylate have problems such as insufficient catalytic activity, high costs, high operational risks, and the lack of efficient and stable catalysts.

Method used

A nano-supported gold-iridium catalyst is used, which is made of gold, iridium, magnesium-based and aluminum-based materials. By regulating the alkaline active site and structure of the carrier, a catalyst with an average particle size of 1.5nm is prepared, taking advantage of the synergy of gold and iridium. It improves catalytic activity and reduces costs through simplified preparation processes.

Benefits of technology

High conversion rate and high selectivity are achieved. The conversion rate of the catalyst to methacrolein reaches 99%, and the selectivity to methyl methacrylate reaches 99%. The preparation process is simple and suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118122325B_ABST
    Figure CN118122325B_ABST
Patent Text Reader

Abstract

The invention discloses a nano-supported gold-iridium catalyst and a preparation method and application thereof, belonging to the field of catalysts. The catalyst is composed of gold, iridium and a carrier, wherein the gold loading is 2wt% to 3wt%, and the iridium loading is 0.8wt% to 1.0wt%; the carrier is prepared from magnesium-based and aluminum-based materials. First, magnesium-based materials and aluminum-based materials are prepared respectively, mixed evenly in proportion and then sintered into a carrier, iridium salt is added to a chloroauric acid solution and then added to the prepared carrier for wet impregnation and ultrasound, vacuum dried and ground into powder, and finally heated and reduced with hydrogen to obtain a nano-supported gold-iridium catalyst. The catalyst of the invention can be used in the preparation of methyl methacrylate by oxidative esterification of methacrolein, with a methacrolein conversion rate of 98% and a methyl methacrylate selectivity of up to 99%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalysts, and in particular to a nano-supported gold-iridium catalyst and a preparation method thereof, as well as application of the catalyst in preparing methyl methacrylate by oxidative esterification of methacrolein. Background Art

[0002] Methyl methacrylate (MMA) is an important organic chemical raw material, widely used in chemical industry, aviation, building materials, machinery and electronics. According to the number of carbon atoms in the raw materials, the MMA production process can be divided into three process routes: C2, C3 and C4. my country's MMA production technology started late, and currently only the ACH process and C4 process are in production. The ACH method uses highly toxic hydrocyanic acid as a raw material, and the concentrated sulfuric acid used in the reaction is highly corrosive to the equipment. This method has high technical requirements for equipment, many by-products, high recycling costs, and cumbersome and lengthy processes. The increasing environmental pressure has limited the expansion of the ACH process production scale. In recent years, the C4 route has achieved a technological breakthrough in China. This process uses petroleum by-products as raw materials, and its production capacity has increased year by year.

[0003] At present, some studies have shown that Au-based catalysts have excellent catalytic performance in oxidation or one-step oxidative esterification. It is recorded in the published literature that the multiphase catalysts for one-step oxidative esterification of aldehydes (alcohols) are mostly supported by Al2O3, TiO2, CeO2, Ga2O3, SiO2, polymers, etc., in which the addition of alkaline substances such as NaOH, KOH, and Na2CO3 to the system helps metal or multivalent state technology to obtain higher catalytic activity. For example, Hayashi et al. of Japan Catalyst Company studied the catalytic performance of supported gold catalysts in the oxidative esterification of ethylene glycol (EG) to methyl glycolate (MGC) from 2002 to 2006. It was found that the supported gold catalysts of 1 to 5 nm showed high selectivity in the reaction, which was different from other precious metals (such as Pd, Ru, etc.). It was inferred that gold catalysts have great application potential in oxidative esterification reactions. In 2013, Suzuki et al. of Asahi Kasei Corporation in Japan loaded AuNiOx nanoparticles on composite oxide carriers such as SiO2-Al2O3-MgO, and used gold catalysts for the first time in the reaction of MAL oxidative esterification to MMA. Han et al. studied and prepared a Au-Ni bimetallic catalyst (Au-Ni / LaMg-FDU-12) loaded on ultra-large mesoporous silica (FDU-12) modified with lanthanum and magnesium elements. Through comparative experiments, it was found that the Au-Ni bimetallic catalytic system loaded on FDU-12 with La and Mg elements added at the same time had better activity and selectivity than single metal Au or single metal Ni, while its activity and selectivity were relatively low when La or Mg elements were added alone. Wang Ye's research group studied the catalytic performance of nano-gold catalysts supported on different carriers (including SiO2, SBA-15, Al2O3, TiO2, ZrO2, ZnO, CeO2, MgO, hydrotalcite, and hydroxyapatite) in the oxidative esterification of MAL to MMA. Comparison found that there is a huge correlation between the basic positions of the carrier, especially the strong basic positions, and the reaction activity. Nano-gold catalysts supported on MgO and hydrotalcite (HT) with more strong basic positions showed the best activity in the reaction.

[0004] In recent years, many patents have disclosed new catalyst approaches for preparing methyl methacrylate, especially the preparation of catalysts for oxidative esterification reactions using methanol and methacrolein as raw materials.

[0005] Chinese Patent No. 202011277177.8 discloses a gold-based catalyst for preparing carboxylic acid esters by oxidative esterification and its application. It discloses that gold is used as the main active ingredient, aluminum hydroxide is used as the carrier, and the gold particle size is less than 8nm. The prepared catalyst has obvious catalytic activity, and the conversion rate of MAL is as high as 96.6%, and the selectivity for MMA is as high as 91.9%. However, in this technical solution, the particle size of gold is still large, and its catalytic activity is still greatly improved. In addition, the gold content of the catalyst is high, resulting in excessive cost of the catalyst.

[0006] Chinese patent CN108607550A discloses a gold catalyst for producing methyl methacrylate, wherein SiO2-A12O3 is used as a carrier, silica sol is used as a precursor, alkaline earth metals are used as co-catalysts, spray drying is used for molding, and gold particles are loaded by impregnation.

[0007] Chinese patent CN105722816A discloses a method for preparing methyl methacrylate by directly oxidizing and esterifying methacrolein with oxygen and methanol. The catalyst used is a gold catalyst supported on SiO2-Al2O3-MgO. However, this method requires the addition of additional alkali to control the pH value of the reaction solution to achieve the purpose of promoting esterification, which involves certain operational risks.

[0008] Although the prior art has proposed a variety of gold-based catalysts for producing methyl methacrylate, there is still a need to provide a high-efficiency gold-containing catalyst for producing methyl methacrylate, which has high product selectivity, raw material conversion rate and stability. Summary of the invention

[0009] The purpose of the present invention is to provide a nano-supported gold-iridium catalyst with high dispersibility, good reaction selectivity and high conversion rate, and to provide a preparation method of the catalyst, the preparation process is simple and does not use organic ligands or add alkali, so as to be suitable for industrial production; and to provide the use of the nano-supported gold-iridium catalyst in the oxidative esterification of methacrolein to prepare methyl methacrylate, so as to solve the technical problems mentioned in the above background technology.

[0010] In order to solve the above technical problems, the technical solutions of the present invention are as follows:

[0011] One purpose of the present invention is to provide a nano-supported gold-iridium catalyst, which is composed of gold, iridium and a carrier, wherein the gold loading is 2wt% to 3wt%, and the iridium loading is 0.8wt% to 1.0wt%; the carrier is prepared from magnesium-based and aluminum-based materials in a molar ratio of (2-4):1.

[0012] Preferably, the gold is metallic elemental gold or a multivalent gold salt, and the multivalent gold salt is one of chloroauric acid and potassium chloroaurate.

[0013] Preferably, the iridium is one of iridium chloride, chloroiridic acid, iridium acetate or sodium chloroiridate hexahydrate.

[0014] Another object of the present invention is to provide a method for preparing the nano-supported gold-iridium catalyst, the specific steps of which are as follows:

[0015] (1) dissolving magnesium salt in ultrapure water to prepare a magnesium salt solution with a concentration of 1.0 g / mL, adding ammonia water twice the amount of the magnesium salt dropwise to the magnesium salt solution, stirring at room temperature for 2 hours, filtering after cooling, washing with ultrapure water for 3 times, drying in an oven at 70° C. for 12 hours, and then placing in a muffle furnace, heating to 340-350° C. at a heating rate of 5° C. / min, and maintaining for 2 hours to obtain a magnesium-based material;

[0016] The obtained carrier was subjected to thermogravimetric analysis. When the heating temperature was between 340-350°C, a mixture of Mg(OH)2 and MgO was obtained. In this step, the solid alkali magnesium oxide-magnesium hydroxide composition was regulated by adjusting the heating temperature, and the alkali content was increased to make it more dispersible. The average particle size of Au and Ir was 1.5 nm, which could effectively improve the MAL selective oxidation MMA performance.

[0017] (2) dissolving aluminum salt in ultrapure water to prepare an aluminum salt solution with a concentration of 1.0 g / mL, adding ammonia water 3 times the amount of the aluminum salt dropwise to the aluminum salt solution, stirring at room temperature for 2 h, filtering after cooling, washing with ultrapure water 3 times, drying in an oven at 50° C. for 12 h, and then placing in a muffle furnace, heating to 320° C. at a heating rate of 5° C. / min, and maintaining for 2 h to obtain an aluminum-based material;

[0018] (3) mixing the magnesium-based material and the aluminum-based material in a molar ratio of (2-4):1, and then placing the mixture in a muffle furnace, heating the mixture to 300°C at a heating rate of 5°C / min, and maintaining the mixture for 2 hours to obtain a carrier;

[0019] (4) Take an iridium salt and add it to a chloroauric acid solution, add it to the prepared carrier for wet impregnation, stir at room temperature for 2 hours, then ultrasonicate for 1 hour, put it in a vacuum drying oven at 50°C for 3 hours, pour it into a mortar and grind it into powder, wash it with ultrapure water until no chloride ions are detected, and then place it in a reduction furnace under a H2 atmosphere, heat it to 200-240°C at a heating rate of 5°C / min for reduction for 2 hours, take it out and grind it with a nano grinder to obtain a nano-supported gold iridium catalyst.

[0020] In the above preparation process, the calcination temperature in the preparation of the magnesium-based material is regulated to adjust the composition ratio of magnesium oxide-magnesium hydroxide in the magnesium-based material, increase the content of alkali, and make it have better alkali active sites. At the same time, the magnesium-based material and the aluminum-based material are mixed and sintered to make the carrier have a three-dimensional porous structure, so that the carrier has a three-dimensional structure with more alkaline active sites, and form a synergistic effect, thereby greatly improving the catalytic activity of the catalyst. In addition, in the final grinding process, a nano-grinder is used for grinding, so that the average particle size of the catalyst is 1.5nm, thereby greatly improving the catalyst's performance in selective oxidation of MMA by MAL.

[0021] Preferably, in step (1), the magnesium salt is one of magnesium chloride, magnesium nitrate and magnesium sulfate.

[0022] Preferably, in step (2), the aluminum salt is one of aluminum chloride, aluminum sulfate and aluminum nitrate.

[0023] Preferably, in step (4), the molar ratio of iridium salt to chloroauric acid is (0.8-1.0):(2-3).

[0024] Preferably, in step (2), the concentration of the chloroauric acid solution is 0.1-0.2 g / mL.

[0025] Another object of the present invention is to provide a method for preparing a nano-supported gold-iridium catalyst, and to use the nano-supported gold-iridium catalyst prepared by the method in the oxidative esterification of methacrolein to prepare methyl methacrylate.

[0026] The nano-supported gold-iridium catalyst was tested in the process of catalyzing the oxidative esterification of methacrolein to prepare methyl methacrylate using the following steps:

[0027] (1) In a sealed stainless steel autoclave, anhydrous methanol, the catalyst of the present invention and MAL were added successively, the mass ratio of methanol to MAL was 30:1, the mass of the catalyst was 0.5 g, and the autoclave was sealed first and then tested for its air tightness;

[0028] (2) introducing oxygen, slowly filling and releasing the gas three times to raise the pressure in the autoclave to 2 atm, and rapidly heating to 70°C and maintaining for 2 h;

[0029] (3) After the reaction stops, turn off the heating, stop stirring, and quickly put it into ice water to cool down. After waiting for 30 minutes, the temperature in the autoclave drops to room temperature, reduce the pressure and take samples, then add ethanol as an internal standard to the reaction solution and stir it. Filter the solution and store it in a vial for detecting the reaction results.

[0030] In the technical scheme of the present invention, the one-step oxidation esterification reaction of methacrolein in an O2 atmosphere mainly includes two processes, oxidation and esterification. Generally, the noble metal active sites activate oxygen molecules to further oxidize aldehyde groups, and the alkaline active sites further esterify the oxidized aldehyde groups to form methyl methacrylate. Therefore, the size of the noble metal, as well as the synergistic effect of the alkaline active sites, metals and carriers in the system, are key factors for the one-step oxidation esterification of methacrolein to methyl methacrylate. In the catalytic process of the present invention, the basic mechanism is that the gold and iridium active sites cooperate with each other to greatly increase the rate of oxidation of aldehyde groups by oxygen molecules, and then the esterification efficiency is further improved through the mutual synergistic promotion of the alkaline active sites of magnesium and aluminum. Moreover, since the structure of the alkaline active sites of magnesium and aluminum is a three-dimensional porous structure, its catalytic efficiency is much greater than that of a single aluminum-based material or magnesium-based material.

[0031] The calculation method of catalytic performance is:

[0032]

[0033]

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. The nano-supported gold-iridium catalyst prepared by the present invention not only has high dispersibility of gold and iridium by regulating the composition of the dual basic active sites and the basic active sites of the carrier itself, but also has an average particle size of 1.5 nm, and the metal and the carrier have a strong synergistic effect, so that the catalyst has a high catalytic conversion rate for methacrolein, good product selectivity, and stronger stability.

[0036] 2. The preparation method of the catalyst of the present invention has easy-to-obtain raw materials, a simple preparation process, and no organic matter is added during the preparation process, which is more suitable for industrial mass production. During the preparation process of the catalyst, when the heating temperature is 345°C and the hydrogen reduction temperature when obtaining the catalyst is 300°C, the activity and product selectivity of the obtained catalyst are the best.

[0037] 3. The nano-supported gold-iridium catalyst of the present invention is applied in the production of methyl methacrylate by oxidative esterification of methacrolein. The conversion rate of methacrolein by the catalyst reaches 99%, and the selectivity of methyl methacrylate reaches up to 99%. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a transmission electron microscopy image of the catalyst prepared in Example 1.

[0039] The structure of the catalyst in the figure is in the form of a three-dimensional porous structure carrier, and there are active sites of Au and Ir on the surface of the structure. DETAILED DESCRIPTION

[0040] The following is a combination of multiple embodiments and comparative examples to verify the preparation process of the catalyst of the present invention and the influencing factors of the preparation parameters, and then further illustrate the technical solution of the invention.

[0041] Example 1

[0042] Preparation of Nano-Supported Gold-Iridium Catalyst

[0043] (1) dissolving magnesium chloride in 50 mL of ultrapure water to prepare a magnesium salt solution with a concentration of 1.0 g / mL, adding ammonia water in an amount twice that of the magnesium salt dropwise to the magnesium salt solution, stirring at room temperature for 2 h, filtering after cooling, washing with ultrapure water for 3 times, drying in an oven at 70° C. for 12 h, and then placing in a muffle furnace, heating to 345° C. at a heating rate of 5° C. / min, and maintaining for 2 h to obtain a magnesium-based material;

[0044] (2) dissolving aluminum chloride in 50 mL of ultrapure water to prepare an aluminum salt solution with a concentration of 1.0 g / mL, adding dropwise an ammonia solution 3 times the amount of the aluminum salt to the aluminum salt solution, stirring at room temperature for 2 h, filtering after cooling, washing with ultrapure water 3 times, drying in an oven at 50° C. for 12 h, and then placing in a muffle furnace, heating to 320° C. at a heating rate of 5° C. / min, and maintaining for 2 h to obtain an aluminum-based material;

[0045] (3) mixing the magnesium-based material and the aluminum-based material in a molar ratio of 3:1, and then placing the mixture in a muffle furnace, heating the mixture to 300° C. at a heating rate of 5° C. / min, and maintaining the mixture for 2 h to obtain a carrier;

[0046] (4) Take iridium chloride and add it to 10 mL of chloroauric acid solution, the concentration of the chloroauric acid solution is 0.15 g / mL, the molar ratio of iridium salt to chloroauric acid is 1:2.5, add it to the prepared 2 g carrier for wet impregnation for 2 hours, then ultrasonicate for 3 hours, put it in a vacuum drying oven at 50°C for 3 hours, pour it into a mortar and grind it into powder, wash it with ultrapure water until no chloride ions are detected, and then place it in a reduction furnace under H2 atmosphere, heat it to 220°C at a heating rate of 5°C / min for reduction for 2 hours, take it out and grind it with a nano grinder to obtain a nano-supported gold iridium catalyst.

[0047] Example 2

[0048] Compared with Example 1, Example 2 of the present invention is different in that in step (1), the magnesium-based material is prepared by placing it in a muffle furnace, heating it to 340° C. at a heating rate of 5° C. / min, and maintaining it for 2 hours to finally prepare a supported gold-iridium catalyst.

[0049] Example 3

[0050] Compared with Example 1, Example 2 of the present invention is different in that in step (1), the magnesium-based material is prepared by placing it in a muffle furnace, heating it to 350° C. at a heating rate of 5° C. / min, and maintaining it for 2 hours to finally prepare a supported gold-iridium catalyst.

[0051] Example 4

[0052] Compared with Example 1, Example 4 of the present invention is different in that in step (3), the magnesium-based material and the aluminum-based material are evenly mixed in a molar ratio of 2:1 to finally prepare a supported gold-iridium catalyst.

[0053] Example 5

[0054] Compared with Example 1, Example 5 of the present invention is different in that in step (3), the magnesium-based material and the aluminum-based material are evenly mixed in a molar ratio of 4:1 to finally prepare a supported gold-iridium catalyst.

[0055] Example 6

[0056] Compared with Example 1, Example 6 of the present invention is different in that the concentration of the chloroauric acid solution in step (4) is 0.1 mg / mL, and a supported gold-iridium catalyst is finally prepared.

[0057] Example 7

[0058] Compared with Example 1, Example 7 of the present invention is different in that the concentration of the chloroauric acid solution in step (4) is 0.2 mg / mL, and a supported gold-iridium catalyst is finally prepared.

[0059] Example 8

[0060] Compared with Example 1, Example 8 of the present invention is different in that the molar ratio of iridium salt and chloroauric acid in step (4) is 1:2 and added to the prepared carrier for wet impregnation for 2 hours to finally prepare a supported gold-iridium catalyst.

[0061] Example 9

[0062] Compared with Example 1, Example 8 of the present invention is different in that the molar ratio of iridium salt and chloroauric acid in step (4) is 1:3, which is added to the prepared carrier for wet impregnation for 2 hours to finally prepare a supported gold-iridium catalyst.

[0063] Example 10

[0064] Compared with Example 1, Example 10 of the present invention is different in that in step (4), the material is placed in a reduction furnace under a H2 atmosphere, heated to 200°C at a heating rate of 5°C / min and reduced for 2h to finally prepare a supported gold-iridium catalyst.

[0065] Embodiment 11

[0066] Compared with Example 1, Example 10 of the present invention is different in that in step (4), the catalyst is placed in a reduction furnace under a H2 atmosphere, heated to 240°C at a heating rate of 5°C / min and reduced for 2 hours to finally prepare a supported gold-iridium catalyst.

[0067] Comparative Example 1

[0068] The difference between Comparative Example 1 of the present invention and Example 1 is that no iridium chloride is added in step (4), and a supported gold-iridium catalyst is finally prepared.

[0069] Comparative Example 2

[0070] Compared with Example 1, Comparative Example 2 of the present invention is different in that no chloroauric acid solution is added in step (4), and a supported gold-iridium catalyst is finally prepared.

[0071] Comparative Example 3

[0072] Compared with Example 1, Comparative Example 3 of the present invention is different in that no aluminum-based material is prepared and step (3) is not performed, and a supported gold-iridium catalyst is finally prepared.

[0073] Comparative Example 4

[0074] Compared with Example 1, Comparative Example 4 of the present invention is different in that no magnesium-based material is prepared and step (3) is not performed, and a supported gold-iridium catalyst is finally prepared.

[0075] The components of the carriers prepared in Examples 1 to 11 and Comparative Examples 1 to 4 were tested and analyzed, and the activity of the nano-supported gold-iridium catalyst in catalyzing the oxidative esterification of methacrolein was tested.

[0076] In a 50mL sealed stainless steel autoclave, anhydrous methanol, gold-iridium catalyst and MAL were added successively, and the airtightness was tested first. Then oxygen was introduced, and the air was slowly filled and discharged three times to raise the pressure in the autoclave to 2atm, and the temperature was quickly heated to 70℃ and maintained for 2h; after the reaction stopped, the heating was turned off, the stirring was stopped, and the autoclave was quickly placed in ice water to cool down. After waiting for 30min, the temperature in the autoclave dropped to room temperature, and the pressure was reduced and sampled. Then ethanol was added to the reaction solution as an internal standard and stirred. The solution was filtered and stored in a vial for detecting the reaction results.

[0077] Conventional activity evaluation conditions are: methanol to MAL mass ratio of 30:1, catalyst mass 0.5 g, oxygen pressure 2 atm, reaction temperature 70 ° C, reaction time 2 h.

[0078] Catalytic performance test and calculation method: After the reaction is completed, 0.5 mL of anhydrous ethanol is added to the reaction solution, and then the reaction solution is detected using an Agilent GC-8890 gas chromatograph.

[0079] Through the performance test and calculation method of the catalyst obtained in the above examples, the conversion rate of the catalyst to MAL and the selectivity to MMA in Table 1 can be obtained.

[0080] Table 1 Effect of the catalysts obtained from different examples on the performance of catalytic MAL to MMA

[0081]

[0082] It can be seen from the data in Table 1 that the catalysts prepared in different embodiments of the present invention have different effects on the performance of MAL to MMA. From the above data, it can be concluded that:

[0083] (1) It can be seen from Examples 1 to 3 that when the calcination temperature of the magnesium-based material is 345°C, a catalyst with optimal catalytic performance can be obtained. If the temperature is too high or too low, the ratio of MgO and Mg(OH)2 in the magnesium-based material will change, thereby reducing the activity of the catalyst.

[0084] (2) It can be seen from Example 1, Example 4, Example 5, Comparative Example 3 and Comparative Example 4 that when the molar ratio of magnesium-based material to aluminum-based material is 3:1, the catalytic activity of the catalyst is the highest; at the same time, the magnesium-based and aluminum-based materials can play a synergistic role to further improve the catalytic activity of the catalyst.

[0085] (3) It can be seen from Example 1, Example 6 and Example 7 that when the concentration of chloroauric acid solution is 0.15 mmol / L, the catalytic activity of the catalyst is the highest.

[0086] (4) It can be seen from Example 1, Example 8, Example 9, Comparative Example 1 and Comparative Example 2 that when the molar ratio of iridium chloride to chloroauric acid is 1:2.5, the catalytic activity of the catalyst is the highest.

[0087] (5) It can be seen from Example 1, Example 10 and Example 11 that the catalytic activity of the catalyst is highest when the temperature of the final heating reduction in hydrogen is 220°C.

[0088] In summary, the catalyst of the present invention has the highest catalytic activity when the calcination temperature of the magnesium-based material is 345°C, the molar ratio of the magnesium-based material to the aluminum-based material is 3:1, the concentration of the chloroauric acid solution is 0.15 mmoL, the molar ratio of the iridium salt to the chloroauric acid is 1:2.5, and the heating reduction temperature in hydrogen is 220°C. The MAL conversion rate reaches 98%, and the MMA selectivity reaches 99%.

[0089] In addition, in the technical solution of the present invention, during the preparation process of the catalyst, not only the catalytic performance of magnesium chloride and aluminum chloride is studied and tested, but also the catalytic performance of the catalyst prepared using nitrates and sulfates of magnesium and aluminum is studied, and the activity of the catalyst is evaluated, so as to study the catalytic performance of different metal salts on the catalyst.

[0090] Example 12

[0091] Compared with Example 1, Example 12 of the present invention is different in that the magnesium salt in step (1) is magnesium nitrate, and the aluminum salt in step (2) is aluminum nitrate to prepare the catalyst.

[0092] Example 13

[0093] Compared with Example 1, Example 13 of the present invention is different in that the magnesium salt in step (1) is magnesium sulfate, and the aluminum salt in step (2) is aluminum sulfate to prepare the catalyst.

[0094] The examples 12 and 13 were experimentally verified, and the conversion rate of the catalyst to MAL and the selectivity to MMA were calculated, as shown in Table 2.

[0095] Table 2 Catalytic performance of catalysts prepared from different aluminum salts and magnesium salts

[0096]

[0097] From the data in Table 2, it can be seen that whether using magnesium salts and aluminum salts of chlorate, nitrate or sulfate, the catalytic performance of the catalyst is not significantly affected. It can be concluded that in the preparation process of the catalyst, the selection of iridium salt also has little effect on the catalytic performance of the catalyst.

Claims

1. A nano-supported gold-iridium catalyst, It is characterized in that The catalyst is composed of gold, iridium and a carrier, wherein the loading amount of gold is 2wt% to 3wt%, and the loading amount of iridium is 0.8wt% to 1.0wt%; the carrier is prepared from magnesium-based and aluminum-based materials in a molar ratio of (2-4):1; The specific preparation steps of the catalyst are as follows: (1) Dissolve magnesium salt in ultrapure water to prepare a magnesium salt solution with a concentration of 1.0 g / mL, add ammonia water twice the amount of magnesium salt dropwise to the magnesium salt solution, stir at room temperature for 2 hours, filter after cooling, wash with ultrapure water for 3 times, dry in an oven at 70°C for 12 hours, and then place in a muffle furnace, heat to 340-350°C at a heating rate of 5°C / min, and maintain for 2 hours to obtain a magnesium-based material; (2) Dissolve aluminum salt in ultrapure water to prepare an aluminum salt solution with a concentration of 1.0 g / mL, add ammonia water 3 times the amount of the aluminum salt dropwise to the aluminum salt solution, stir at room temperature for 2 hours, filter after cooling, wash with ultrapure water 3 times, dry in an oven at 50°C for 12 hours, then place in a muffle furnace, heat to 320°C at a heating rate of 5°C / min, and maintain for 2 hours to obtain an aluminum-based material; (3) The magnesium-based material and the aluminum-based material are uniformly mixed in a molar ratio of (2-4):1, and then placed in a muffle furnace, heated to 300°C at a heating rate of 5°C / min, and maintained for 2 hours to obtain a carrier; (4) Take iridium salt and add it to chloroauric acid solution, add it to the prepared carrier and wet-immerse it for 2 hours, then ultrasonicate it for 1 hour, put it in a vacuum drying oven at 50°C and dry it for 3 hours, pour it into a mortar and grind it into powder, wash it with ultrapure water until no chloride ions are detected, and then place it in H 2 In a reduction furnace under an atmosphere, the mixture was heated to 200-240°C at a heating rate of 5°C / min and reduced for 2 hours. After being taken out, the mixture was ground with a nano-grinder to obtain a nano-supported gold-iridium catalyst.

2. The nano-supported gold-iridium catalyst according to claim 1, wherein the gold is metal elemental gold or a multivalent gold salt, and the multivalent gold salt is one of chloroauric acid and potassium chloroaurate.

3. The nano-supported gold-iridium catalyst according to claim 1, It is characterized in that, The iridium is one of iridium chloride, chloroiridic acid, iridium acetate or sodium chloroiridate hexahydrate.

4. According to the nano supported gold iridium catalyst described in claim 1, It is characterized in that In the step (1), the magnesium salt is one of magnesium chloride, magnesium nitrate and magnesium sulfate.

5. According to the nano supported gold iridium catalyst described in claim 1, It is characterized in that In the step (2), the aluminum salt is one of aluminum chloride, aluminum sulfate and aluminum nitrate.

6. According to the nano-supported gold-iridium catalyst described in claim 1, It is characterized in that In the step (4), the molar ratio of the iridium salt to the chloroauric acid is (0.8-1.0):(2-3).

7. According to the nano-supported gold-iridium catalyst described in claim 1, It is characterized in that In the step (2), the concentration of the chloroauric acid solution is 0.1-0.2 g / mL.

8. Use of the nano-supported gold-iridium catalyst according to any one of claims 1 to 7 in the preparation of methyl methacrylate by oxidative esterification of methacrolein.