Crop straw activation method, application and lithium battery made therefrom
By carbonizing, calcining and modifying crop straw, porous carbon with a high specific surface area is prepared, which solves the problems of high cost and low performance of lithium battery electrode materials, improves the performance and reduces the cost of lithium batteries, and has good Industrial application value.
Patent Information
- Application Number
- CN202410544400.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-05-06
AI Technical Summary
The manufacturing cost of existing lithium battery electrode materials is high, and supercapacitor carbon has low specific capacitance and large internal resistance, mainly due to small specific surface area, fewer micropores and mesopores, and lacks high value-added methods for utilizing crop straw.
By turbine grinding, carbonizing, calcining, purifying and modifying crop straw, porous carbon with high specific surface area and rich pore structure is prepared, and combined with aminobenzene, 1-aza-2,4- in lithium batteries Chemical substances such as cyclopentadiene, hydrogen peroxide and azobisisobutyronitrile form composite porous carbon to improve electrical conductivity.
It significantly improves the specific capacitance and conductivity of lithium batteries, reduces battery costs, has both environmental and economic benefits, and has good promotion and industrial application value.
Smart Images

Figure CN118125440B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of development of new energy materials and resource utilization of solid waste, and relates to a crop straw activation method, application and lithium battery manufactured therefrom. Background Art
[0002] Energy is the core driving force for economic development, and it is also the main bottleneck restricting economic development. At present, the mainstream energy storage devices are mainly lithium batteries and supercapacitors, and their core is electrode materials, but the manufacturing cost of key electrode materials is high. Achieving technological breakthroughs in the processing and utilization of energy storage materials and reducing the cost of electrode materials for energy storage are the key to the industrialization of energy storage. Carbon materials have become the preferred electrode material due to their advantages such as good conductivity, mechanical stability and low cost. Supercapacitor carbon can be used in new energy storage devices such as supercapacitors and lithium batteries, and then in new energy vehicles, wind power generation and other fields. The core of supercapacitors is carbon materials. At present, the main activation method is mainly based on single alkali activation. Supercapacitor carbon prepared by this activation method generally has problems such as low specific capacitance and large internal resistance. The reason is mainly due to the small specific surface area and fewer micropores and mesopores.
[0003] During the harvest season every year, crops will produce a large amount of discarded straw, which is used in a relatively simple way, mainly as soil fertilizer and poultry feed. There is a lack of high value-added utilization methods, so it is urgent to develop high value-added utilization methods for straw. This patent uses the straw of different crops as raw materials and prepares high-value-added high-quality energy storage electrode materials through a specific process. Summary of the invention
[0004] The purpose of the present invention is to provide a crop straw activation method, application and lithium battery manufactured therefrom. The manufactured lithium-ion battery not only has excellent conductive properties, but also has both environmental and economic benefits, and has good promotion and industrial application value.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for activating crop straw comprises the following steps:
[0007] Step 1: The straw is crushed by a turbine grinder and passed through an 80-120 mesh sieve, and then transferred to a tubular furnace and carbonized at a temperature of 600-800°C for 1-3 hours to prepare porous carbon with a porous structure, and the obtained porous carbon is passed through a 180-200 mesh sieve; then added to a grinding device together with potassium hydroxide and potassium bicarbonate for sufficient grinding; after grinding, the obtained mixed powder is transferred to a high-temperature tubular furnace and calcined at a high temperature of 500-800°C for 1-3 hours; after calcination, it is purified and modified in turn; the obtained modified porous carbon is stored and reserved;
[0008] Step 2, the modified porous carbon is put into a 1.0-1.5 mol / L hydrochloric acid solution at a solid-liquid ratio of 0.01-0.03 g / mL, and then aminobenzene and 1-aza-2,4-cyclopentadiene are added in turn, which are 0.6-1.0 times the mass of the modified porous carbon. After ultrasonic dispersion for 2-3 hours, hydrogen peroxide and 0.06-0.1 times the mass of the modified porous carbon are added to the obtained mixed components in sequence under nitrogen protection. After mixing and stirring evenly, the temperature is raised to 70-90°C, and the reaction is kept at this temperature for 5-18 hours; after the reaction is completed, the obtained product components are filtered, the obtained filter cake is washed with hydrochloric acid for 4-5 times, and then washed with deionized water until the filtrate is colorless, and then vacuum dried to obtain a composite porous carbon.
[0009] Furthermore, in the step 1, the mass ratio of the porous carbon, potassium hydroxide and potassium bicarbonate is 1-5:1-1.5:1-1.5.
[0010] Furthermore, the specific steps of the purification process in step 1 are: transferring the calcined mixed powder into a reactor, adding a purification solution 5 to 8 times the mass of the mixed powder, ultrasonically dispersing for 20 to 30 minutes and then filtering it, washing the obtained filter cake with deionized water until it is neutral, and then vacuum drying it.
[0011] Furthermore, the purification solution is prepared by mixing hydrofluoric acid and ethanol in a volume ratio of 2 to 5:1; wherein the concentration of hydrofluoric acid is 5 to 6 mol / L.
[0012] Furthermore, the straw used in step 1 is any one of rice straw, wheat straw and corn straw.
[0013] Furthermore, the carbon content of rice straw is 48-50%, and the density is about 0.9-1.2 g / cm 3 ;
[0014] The carbon content of wheat straw is 45-46%, and the density is about 0.8-0.9 g / cm 3 ;
[0015] Corn stalks contain 30-35% carbon and have a density of about 0.7-0.8 g / cm 3 .
[0016] Furthermore, the preparation method of the modified porous carbon is as follows: the porous carbon is put into a 5-8 mol / L nitric acid solution at a solid-liquid ratio of 20-40 g / L, mixed and stirred evenly, and then kept warm for reaction at a temperature of 70-85° C. for 8-15 hours; after the reaction is completed, the product components are filtered, washed and dried in turn; the obtained solid material is put into thionyl chloride at a solid-liquid ratio of 0.005-0.01 g / mL, ultrasonically dispersed for 30-50 minutes, and then refluxed for 8-12 hours; after the reaction is completed, the residual thionyl chloride in the product is evaporated, and the result is the modified porous carbon.
[0017] Furthermore, in the step 2, the vacuum drying temperature is 50-70° C., and the vacuum drying time is 40-50 hours.
[0018] The second object of the present invention is to provide a method for activating crop straw and use it in manufacturing lithium batteries.
[0019] A third object of the present invention is to provide a method for manufacturing a lithium battery, comprising the following steps:
[0020] S1. 0.3 g of the above-mentioned composite porous carbon, 4.5 g of stannous chloride, 0.8 g of graphite and 2 mL of concentrated HCl were added to 150 mL of water and stirred rapidly, and then 6 mL of formic acid was slowly dropped, and refluxed at 100° C. for 6 h; after the reaction was completed, the components of the product were separated, washed and dried in turn; then nitrogen was introduced into the obtained mixture, and heat-treated at 600° C. for 1 h, and cooled naturally;
[0021] S2, 0.4g of the mixture prepared in step S1, 0.05g of acetylene black and 0.05g of polyvinylidene fluoride PVDF were mixed and stirred evenly, and then 1mL of N-methylpyrrolidone was added, and the mixed slurry was evenly coated on the copper foil after mixing and grinding evenly, and the coating thickness was 60μm; then the obtained electrode was vacuum dried at a temperature of 100°C for 8h; after drying, it was pressed into a sheet;
[0022] S3, using lithium metal sheet as counter electrode, polypropylene film as diaphragm, and a mixture of LiPF6, EC and DMC as electrolyte, a lithium-ion battery was made in a glove box; 6 The concentration was 1 mol / L, and the mass ratio of EC to DMC was 1:1.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] 1. The carbonization temperature is controlled within the range of 600-800°C. The porous carbon prepared within this temperature range has a higher carbon mass fraction and more pore structures. A higher carbon mass fraction is beneficial to improving the conductivity of the material, while a more porous structure is beneficial to the preparation of supercapacitor carbon with a high specific surface area.
[0025] 2. The strong corrosiveness of potassium hydroxide is used to etch the carbon material to obtain a larger specific surface area and pore volume. At the same time, the gas produced by the decomposition of potassium bicarbonate at high temperature can play a certain pore expansion effect, which is conducive to obtaining a carbon material with a large specific surface area and rich micropores and mesopores, thereby affecting the specific capacitance and conductivity of the supercapacitor carbon.
[0026] 3. The mixed solution of hydrofluoric acid and ethanol removes impurities such as unstable carbon and metal oxides in the carbon material. The volume ratio and the concentration of hydrofluoric acid affect the degree of reaction, that is, the purity of the carbon material, which in turn affects its electrochemical performance.
[0027] 4. In the present invention, nitric acid solution and thionyl chloride are used for activation treatment to introduce active groups on the surface of porous carbon and in its pore structure. The active groups react chemically with aminobenzene and 1-aza-2,4-cyclopentadiene under the action of azobisisobutyronitrile and hydrogen peroxide to form bonds, and finally form a criss-cross three-dimensional network conductive film layer on its surface and in its pore structure, which significantly improves the conductive properties of the porous carbon and effectively guarantees the performance of the prepared lithium battery product.
[0028] 5. The method provided by the present invention is simple in process, low in energy consumption, and mild in operating conditions. The manufactured battery has good electrochemical performance, both environmental and economic benefits, and has good promotion and industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a SEM image of the composite porous carbon prepared in Example 1 of the present invention;
[0030] Figure 2 The CV curve diagram of the electrochemical performance test of the composite porous carbon prepared in Example 1 of the present invention when used as a carbon material for supercapacitor;
[0031] Figure 3 CV curve of electrochemical performance test of YP80F carbon material for commercial supercapacitors;
[0032] Figure 4 The GCD diagrams of the composite porous carbon prepared in Example 1 of the present invention and the commercially available supercapacitor carbon YP80F at 1 A / g when used as supercapacitor carbon materials respectively;
[0033] Figure 5This is the nitrogen adsorption-desorption curve of the composite porous carbon prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Embodiment 1: A method for activating crop straw, comprising the following steps:
[0036] Step 1: Mix wheat straw and corn straw in a mass ratio of 3:1, grind them with a turbine grinder and pass through an 80-mesh sieve, then transfer them to a tubular furnace and carbonize them at a temperature of 600°C for 1 hour to prepare porous carbon with a porous structure, and the obtained porous carbon passes through a 180-mesh sieve; then add them together with potassium hydroxide and potassium bicarbonate into a grinding device for sufficient grinding; after grinding, transfer the obtained mixed powder to a high-temperature tubular furnace and calcine at 800°C for 3 hours; after calcination, purify and modify them in turn; the obtained modified porous carbon is stored and used for standby;
[0037] Among them, wheat straw contains 45-46% carbon and has a density of about 0.8-0.9 g / cm 3 ; The carbon content of corn stalks is 30-35%, and the density is about 0.7-0.8g / cm 3 ;
[0038] The mass ratio of porous carbon, potassium hydroxide, and potassium bicarbonate is 5:1:1;
[0039] The specific steps of the purification process are: transferring the calcined mixed powder into a reactor, adding a purification solution 5 times the mass of the mixed powder, ultrasonically dispersing it for 20 minutes and then filtering it, washing the obtained filter cake with deionized water until it is neutral, and then vacuum drying it; and the purification solution is prepared by mixing hydrofluoric acid and ethanol in a volume ratio of 2:1; wherein the concentration of hydrofluoric acid is 5 mol / L.
[0040] Step 2: put the modified porous carbon into a 1.0 mol / L hydrochloric acid solution at a solid-liquid ratio of 0.01 g / mL, and then add aminobenzene and 1-aza-2,4-cyclopentadiene in an amount of 0.6 times the mass of the modified porous carbon in sequence. After ultrasonic dispersion for 2 hours, add hydrogen peroxide and azobisisobutyronitrile in an amount of 0.05 times the mass of the modified porous carbon in sequence under nitrogen protection. After mixing and stirring evenly, heat to 70°C and keep at this temperature for reaction for 5 hours. After the reaction is completed, filter the resulting component, wash the filter cake with hydrochloric acid 4 times, and then wash with deionized water until the filtrate is colorless, and then vacuum dry to obtain a composite porous carbon. The vacuum drying temperature is 50°C and the vacuum drying time is 40 hours.
[0041] The preparation method of modified porous carbon is as follows: porous carbon is put into 5 mol / L nitric acid solution at a solid-liquid ratio of 20 g / L, mixed and stirred evenly, and then kept warm for reaction at 70°C for 8 hours; after the reaction is completed, the product components are filtered, washed and dried in turn; the obtained solid material is put into thionyl chloride at a solid-liquid ratio of 0.005 g / mL, ultrasonically dispersed for 30 minutes, and then refluxed for 8 hours; after the reaction is completed, the residual thionyl chloride in the product is evaporated, and the result is modified porous carbon.
[0042] The SEM image of the composite porous carbon prepared in this example is as follows Figure 1 As shown in the figure, it can be seen that the composite porous carbon has a large number of micropores and mesopores, a lamellar structure and obvious pores, which lays the foundation for its good electrochemical performance.
[0043] Example 2: The difference between this example and Example 1 is that this example uses rice straw alone as the raw material for preparing the modified porous carbon, and the carbon content of the rice straw is 48-50%, and the density is about 0.9-1.2 g / cm 3 ;
[0044] The carbonization temperature is 620℃, and the carbonization time is 2h; the high temperature calcination temperature is 700℃, and the calcination time is 3h;
[0045] The mass ratio of porous carbon, potassium hydroxide and potassium bicarbonate is 5:1:1.
[0046] Example 3: The difference between this example and Example 1 is that: in this example, wheat straw is used alone as the raw material for preparing the modified porous carbon; and the carbon content of wheat straw is 45-46%, and the density is about 0.8-0.9 g / cm 3 ;
[0047] The carbonization temperature is 660℃, and the carbonization time is 2h; the high temperature calcination temperature is 600℃, and the calcination time is 2h;
[0048] The mass ratio of porous carbon, potassium hydroxide and potassium bicarbonate is 5:1.5:1.5.
[0049] Example 4: The difference between this example and Example 1 is that in this example, rice straw and corn straw are mixed in a mass ratio of 3:1, and the carbon content of the rice straw is 48-50%, and the density is about 0.9-1.2 g / cm 3 ; The carbon content of corn stalks is 30-35%, and the density is about 0.7-0.8g / cm 3 ;
[0050] The carbonization temperature is 700℃, and the carbonization time is 3h; the high temperature calcination temperature is 500℃, and the calcination time is 1h;
[0051] The mass ratio of porous carbon, potassium hydroxide and potassium bicarbonate is 1:1:1.
[0052] The composite porous carbon products prepared in Examples 2 to 4 all contain a lamellar structure with abundant pore channels, a large specific surface area, and good electrochemical properties.
[0053] Product performance test:
[0054] 1. Materials for supercapacitors: The composite porous carbon prepared in Example 1 was assembled into three electrodes for electrochemical performance testing. The specific assembly process is as follows:
[0055] (1) Weigh 80 mg of the composite porous carbon prepared in Example 1 and 10 mg of the conductive agent acetylene black, and stir the dry powder for 30 min. At the same time, ultrasonically disperse and dissolve 10 mg of polytetrafluoroethylene powder in 1 mL of ethanol to prepare a dispersion. Pour the dry powder after stirring into the dispersion, ultrasonically disperse again for 30 min, and magnetically stir for 8 h, with the speed controlled at 400 r / min;
[0056] (2) Weighing the mass of the nickel sheet, and applying the coating prepared in step (1) onto the nickel sheet;
[0057] (3) Dry the electrode sheet prepared in step (2) under vacuum at 80 °C for 6 h;
[0058] (4) Press the dried electrode sheet into a sheet at a pressure of 15 MPa and weigh it again to obtain the mass of the coating.
[0059] (5) The electrochemical performance of the assembled three-electrode system is tested using conventional methods.
[0060] like Figure 2 As shown in the figure, the CV graph of the composite porous carbon sample prepared in Example 1 is very close to a rectangle, showing good double-layer capacitance characteristics, which is better than Figure 3The CV diagram of commercially available YP80F is shown, which indicates that the cyclability and reversibility of the composite porous carbon sample prepared in Example 1 are better than those of the commercially available YP80F material.
[0061] in addition, Figure 4 The composite porous carbon sample prepared in Example 1 has a specific capacitance of 122 F / g at a current density of 1 A / g, which is 10.9% higher than that of the YP80F material. Moreover, after 10,000 cycles, the specific capacitance retention rates of the composite porous carbon samples prepared in YP80F and Example 1 are 98.5% and 97.9%, respectively, indicating that the composite porous carbon sample prepared in Example 1 has good cycle stability.
[0062] The activation modification method used in the present invention prepares supercapacitor carbon with superior performance, because the composite porous carbon sample prepared in Example 1 produces a large number of micropores and mesopores, the micropores are conducive to the increase of the material's specific capacitance, and the mesopores are conducive to improving the material's conductivity. In addition, during the purification process, the removal of ash oxide impurities and the adjustment of the degree of graphitization improve the conductivity and cycle stability of the supercapacitor carbon material.
[0063]
[0064] 2. Manufacturing lithium battery: A method for manufacturing a lithium battery comprises the following steps:
[0065] S1. Add 0.3 g of the composite porous carbon prepared in the above embodiment, 4.5 g of stannous chloride, 0.8 g of graphite and 2 mL of concentrated HCl into 150 mL of water and stir rapidly, then slowly drop 6 mL of formic acid, and reflux at 100° C. for 6 h; after the reaction is completed, separate, wash and dry the resulting components in turn; then introduce nitrogen into the resulting mixture, heat treat at 600° C. for 1 h, and cool naturally;
[0066] S2, 0.4g of the mixture prepared in step S1, 0.05g of acetylene black and 0.05g of polyvinylidene fluoride PVDF were mixed and stirred evenly, and then 1mL of N-methylpyrrolidone was added, and the mixed slurry was evenly coated on the copper foil after mixing and grinding evenly, and the coating thickness was 60μm; then the obtained electrode was vacuum dried at a temperature of 100°C for 8h; after drying, it was pressed into a sheet;
[0067] S3, with lithium metal sheet as the counter electrode, polypropylene film as the diaphragm, LiPF 6 The mixed solution composed of EC and DMC is used as the electrolyte to make lithium-ion batteries in a glove box; among them, LiPF 6 The concentration was 1 mol / L, and the mass ratio of EC to DMC was 1:1.
[0068] The lithium-ion battery manufactured above has an initial charging capacity of 524 mAh / g, an initial charge and discharge coulombic efficiency of 65.7%, and a capacity of 486 mAh / g after 2000 charge and discharge cycles, with a coulombic efficiency of 92.7%.
[0069] The technical solution provided by the present invention has a simple process, low energy consumption, and mild operating conditions. The manufactured battery has good electrochemical performance, environmental benefits and economic benefits, and has good promotion and industrial application value. This shows that the crop straw activation method, application, and lithium battery manufactured by the present invention have a broader market prospect and are more suitable for promotion.
[0070] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0071] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for activating crop straw, characterized in that: The following steps are involved: Step 1: The straw is crushed by a turbine grinder and passed through a 80-120 mesh sieve, and then transferred into a tubular furnace and carbonized at a temperature of 600-800° C. for 1-3 hours to prepare porous carbon with a porous structure. The obtained porous carbon is passed through a 180-200 mesh sieve; and then added into a grinding device together with potassium hydroxide and potassium bicarbonate for sufficient grinding; After grinding, the obtained mixed powder is transferred to a high-temperature tube furnace and calcined at 500-800°C for 1-3 hours; after calcination, it is purified and modified in turn; The obtained modified porous carbon is stored and used for future use; Step 2, the modified porous carbon is put into a 1.0-1.5 mol / L hydrochloric acid solution at a solid-liquid ratio of 0.01-0.03 g / mL, and then aminobenzene and 1-aza-2,4-cyclopentadiene are added in turn, which are 0.6-1.0 times the mass of the modified porous carbon, and 0.5-0.8 times the mass of the modified porous carbon. After ultrasonic dispersion for 2-3 hours, hydrogen peroxide and 0.06-0.1 times the mass of azobisisobutyronitrile are added to the obtained mixed components in turn under nitrogen protection, and the mixture is mixed and stirred evenly, and then the temperature is raised to 70-90°C, and the reaction is kept at this temperature for 5-18 hours; after the reaction is completed, the obtained product components are filtered, the obtained filter cake is washed with hydrochloric acid for 4-5 times, and then washed with deionized water until the filtrate is colorless, and then vacuum dried to obtain a composite porous carbon; The straw used in step 1 is any one of rice straw, wheat straw and corn straw; The carbon content of rice straw is 48-50%, and the density is 0.9-1.2g / cm 3 ; The carbon content of wheat straw is 45-46%, and the density is 0.8-0.9 g / cm 3 ; Corn stalks contain 30-35% carbon and have a density of 0.7-0.8 g / cm 3 ; The preparation method of the modified porous carbon is as follows: the porous carbon is put into a 5-8 mol / L nitric acid solution at a solid-liquid ratio of 20-40 g / L, mixed and stirred evenly, and then kept warm for reaction at a temperature of 70-85° C. for 8-15 hours; after the reaction is completed, the components of the product are filtered, washed and dried in sequence; the obtained solid material is put into thionyl chloride at a solid-liquid ratio of 0.005-0.01 g / mL, ultrasonically dispersed for 30-50 minutes, and then refluxed for reaction for 8-12 hours; after the reaction is completed, the residual thionyl chloride in the product is evaporated to obtain the modified porous carbon.
2. The method for activating crop straw according to claim 1, characterized in that: In the step 1, the mass ratio of porous carbon, potassium hydroxide and potassium bicarbonate is 1-5:1-1.5:1-1.
5.
3. The method for activating crop straw according to claim 1, characterized in that: The specific steps of the purification process in step 1 are: transferring the calcined mixed powder into a reactor, adding a purification solution 5 to 8 times the mass of the mixed powder, ultrasonically dispersing for 20 to 30 minutes and then filtering it, washing the obtained filter cake with deionized water until it is neutral, and then vacuum drying it.
4. The method for activating crop straw according to claim 3, characterized in that: The purification solution is prepared by mixing hydrofluoric acid and ethanol in a volume ratio of 2 to 5:1; wherein the concentration of hydrofluoric acid is 5 to 6 mol / L.
5. The method for activating crop straw according to claim 1, characterized in that: The vacuum drying temperature in step 2 is 50-70° C., and the vacuum drying time is 40-50 hours.
6. Use of the crop straw activation method according to any one of claims 1 to 5 in manufacturing lithium batteries.
7. A method for manufacturing a lithium battery, characterized in that: The following steps are involved: S1. Add 0.3 g of the composite porous carbon according to any one of claims 1 to 5, 4.5 g of stannous chloride, 0.8 g of graphite and 2 mL of concentrated HCl to 150 mL of water and stir rapidly, then slowly drop 6 mL of formic acid, and reflux at 100°C for 6 h; after the reaction is completed, separate, wash and dry the resulting components in turn; then introduce nitrogen into the resulting mixture, heat treat at 600°C for 1 h, and cool naturally; S2, 0.4g of the mixture prepared in step S1, 0.05g of acetylene black and 0.05g of polyvinylidene fluoride PVDF were mixed and stirred evenly, and then 1mL of N-methylpyrrolidone was added, and the mixed slurry was evenly coated on the copper foil after mixing and grinding evenly, and the coating thickness was 60μm; then the obtained electrode was vacuum dried at a temperature of 100°C for 8h; after drying, it was pressed into a sheet; S3. A lithium-ion battery was produced in a glove box using a metal lithium sheet as the counter electrode, a polypropylene film as the separator, and a mixture of LiPF6, EC and DMC as the electrolyte; the concentration of LiPF6 was 1 mol / L, and the mass ratio of EC to DMC was 1:1.
Citation Information
Patent Citations
Method for using crop straw for treatment of phenol-containing wastewater
CN105293619A
Method for preparing straw-based activated carbon supercapacitor electrode material for enhancing energy storage efficiency through manganese ore
CN110217793A
Activated carbon material applied to supercapacitor electrode material
CN112194133A
Low-temperature activated activated carbon, preparation method and application
CN116375031A
Preparation method of camphor tree seed-based activated carbon for supercapacitor
CN116553539A