A NiFe-based self-supporting electrocatalyst and its preparation method and application
By loading NiFe-LDH hydrotalcite on a conductive substrate and transforming it into a NiFe alloy crystal phase, combined with ultra-thin carbon layer coating, an efficient NiFe-based self-supporting electrocatalyst is formed, which solves the problem of low degradation efficiency of organic pollutants in sewage. It achieves high oxygen reduction activity and degradation ability, reducing costs and recycling problems.
Patent Information
- Application Number
- CN202410457022.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-16
AI Technical Summary
The existing technology has low degradation efficiency of organic pollutants in sewage treatment and insufficient oxygen reduction performance. Moreover, the traditional electro-Fenton method has high energy consumption and high cost, making it difficult to achieve large-scale and efficient treatment.
By hydrophilizing the conductive substrate, the NiFe-LDH hydrotalcite structure is supported, and transformed into the NiFe alloy crystal phase during the pyrolysis process, while coating an ultra-thin carbon layer to form NiFe with high specific surface area and high catalytic activity. self-supporting electrocatalyst.
It improves the oxygen reduction activity and degradation ability of the catalyst, reduces costs, avoids the problem of powder catalyst recycling, and achieves efficient degradation of a variety of organic pollutants.
Smart Images

Figure CN118125568B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of degradation of organic pollutants in sewage, and in particular to a NiFe-based self-supporting electrocatalyst and a preparation method and application thereof. Background Art
[0002] Organic pollutants, such as pharmaceuticals, industrial chemicals, and pesticides, have been widely present in surface water and groundwater, posing a serious threat to the aquatic environment and human health. Although a variety of organic micropollutants exist in low concentrations, most of them tend to be persistent in conventional wastewater treatment processes (WWTP). Social development is ongoing, science and technology are also being updated, and with it comes increasing environmental pollution. In order to effectively solve the problem of water pollution, ensure people's quality of life, and protect ecological security, it is urgent to develop a new technology to effectively treat wastewater.
[0003] Electro-Fenton is an advanced oxidation technology with application prospects developed in recent years in wastewater treatment. Electro-Fenton is based on the ordinary Fenton technology. By adding an external power source, H2O2 is synthesized in situ by oxygen reduction reaction and then activated into active oxygen free radicals to degrade organic matter. It has the advantages of fast reaction speed, easy operation, and environmental friendliness. The application trend of this technology is increasing year by year, and it has been successfully used in wastewater treatment. However, traditional electro-Fenton still faces problems such as low oxygen reduction performance, poor degradation efficiency of organic pollutants, large amounts of iron sludge generated during the reaction, and difficulty in recovering powdered catalysts.
[0004] In order to solve the above technical problems, the prior art mainly proposes the following treatment methods: 1) electrochemical oxidation method, 2) photocatalytic oxidation method, 3) ozone catalytic oxidation method, etc. Among them, the electrochemical oxidation method includes direct electrolytic oxidation method and indirect electrolytic oxidation method. The direct oxidation method is that after the direct current is passed, the anode surface discharge directly generates hydroxyl radicals (·OH) to oxidize the organic pollutants; the indirect oxidation method is to add a salt aqueous solution of a variable valence metal to the electrolytic cell, first form an active group with strong oxidizing properties at the anode, and then use the active group to oxidize the pollutants in the wastewater. That is, although the electrochemical oxidation method can improve the degradation efficiency of organic pollutants in wastewater to a certain extent, the electrochemical oxidation method has high energy consumption and high cost, which is not conducive to promotion and large-scale use. The photocatalytic oxidation method uses semiconductor catalysts to produce ·OH under the irradiation of ultraviolet light, and uses the strong oxidizing effect of ·OH to remove organic pollutants. Although this method can also improve the degradation efficiency of organic pollutants in wastewater to a certain extent, a variety of aromatic organic intermediates will be generated during the treatment process, resulting in incomplete degradation. Ozone itself is a strong oxidant that can oxidize pollutants; however, the hydroxyl radicals produced by its decomposition have stronger oxidizing ability and have better treatment effects than direct ozone oxidation treatment. In addition, the operating cost of ozone catalytic oxidation is relatively high, and pollutants cannot be completely degraded at low doses and in a short period of time. It is also difficult to eliminate the interference of the generated intermediates with the ozone oxidation process.
[0005] Based on the above, it can be seen that the above-mentioned several existing technologies are not conducive to large-scale and efficient degradation of organic pollutants in sewage. To this end, the present invention attempts to provide a NiFe-based self-supporting electrocatalyst and its preparation method and application. Summary of the invention
[0006] In order to solve the deficiencies in the above-mentioned prior art, the present invention provides a NiFe-based self-supporting electrocatalyst and its preparation method and application. The present invention forms a NiFe-LDH hydrotalcite with a unique metal compound sheet array or nanorod array structure on its surface after hydrophilization treatment of the conductive substrate to enhance the specific surface area. Then, by coating dopamine hydrochloride and then performing pyrolysis treatment, an ultra-thin carbon layer is further loaded on the substrate surface, and the NiFe-LDH hydrotalcite is transformed into a NiFe alloy crystal phase during the pyrolysis process, and the sheet structure of the hydrotalcite is retained while being transformed into the NiFe alloy crystal phase, so as to provide an ORR active site through the sheet surface, thereby greatly improving the specific surface area and catalytic activity of the substrate material, so that the obtained NiFe-based self-supporting electrocatalyst has a high specific surface area and high catalytic activity to achieve catalyst structure finalization, enhance oxygen reduction activity and catalytic performance, and then obtain a NiFe-based self-supporting electrocatalyst with the structural characteristics of a metal compound sheet array or a nanorod array.
[0007] A NiFe-based self-supporting electrocatalyst and its preparation method and application of the present invention are achieved through the following technical solutions:
[0008] The first object of the present invention is to provide a method for preparing a NiFe-based self-supporting electrocatalyst, comprising the following steps:
[0009] Step 1, hydrophilization treatment:
[0010] The conductive substrate is subjected to a hydrophilic treatment to obtain a hydrophilic substrate.
[0011] It should be emphasized that the present invention can select different conductive substrates for in-situ loading of NiFe-LDH hydrotalcite materials according to actual needs, such as foam metal or carbon fiber material. Wherein, in a preferred embodiment of the present invention, the foam metal used can be selected from any one of foam nickel, foam copper, and foam iron. In another preferred embodiment of the present invention, the carbon fiber material used can be selected from carbon cloth or carbon felt. In another preferred embodiment of the present invention, considering the wide range of use, good electrical conductivity, high thermal stability, low cost and other factors, carbon cloth is preferably used as the conductive substrate.
[0012] In order to improve the bonding between the conductive substrate and the NiFe-LDH hydrotalcite material in the subsequent process, the present invention firstly performs a hydrophilic treatment on the conductive substrate to improve the adhesion of the conductive substrate, thereby enhancing the bonding or compounding with other materials in the subsequent process.
[0013] In order to ensure that the hydrophilicity of the surface of the conductive substrate can be improved, in a preferred embodiment of the present invention, when a carbon fiber material is used as the conductive substrate, taking carbon cloth as an example, the following method is used to achieve hydrophilic treatment of the conductive substrate of the carbon fiber material:
[0014] The present invention takes into account that the hydrophobic coating on the surface of the carbon cloth causes its poor hydrophilicity, so the cut carbon cloth is first immersed in an alcohol solution to fully infiltrate it, and then boiled at 82-88°C and continued to boil for 15-25 minutes. Since the alcohol solution is a good organic solvent, it can effectively remove the hydrophobic coating on the surface of the carbon cloth. Among them, the alcohol solution used is one or two of ethanol and methanol, and the concentration of the alcohol solution is 99.7%. Then, using acid solution as a treating agent, the boiled and cooled carbon cloth is immersed in the acid solution for ultrasonic treatment, so that the carbon cloth is pickled by ultrasound and acid solution, thereby removing impurities on the surface of the carbon cloth, and modifying oxygen-containing functional groups on the surface of the carbon cloth to improve hydrophilicity. To this end, in another preferred embodiment of the present invention, the acid solution used can be selected from one or more of hydrochloric acid, sulfuric acid and nitric acid, and the ratio of the carbon cloth to the acid solution used during the treatment is 9-16cm 2:30mL; wherein the concentration of the acid solution is 2.5-3.5mol / L. Other substrate materials can also be subjected to corresponding operations in the above manner to achieve the purpose of hydrophilization. It can be understood that since the carbon cloth is impregnated with acid solution, there may be residual acid solution on the surface of the carbon cloth after the impregnation treatment, so the residual acid solution on the surface needs to be washed and removed after the impregnation treatment. In a preferred embodiment of the present invention, deionized water or distilled water is used as a detergent to wash the surface of the carbon cloth, and the pH of the washing liquid is neutral. Then, the residual water on the surface of the carbon cloth is removed by drying, and then the subsequent step 2 is carried out. Among them, the specific method of drying the carbon cloth is not limited, as long as the residual water on the surface of the carbon cloth can be removed.
[0015] When a foam metal is used as a conductive substrate, for example, foam nickel is completely immersed in an alcohol solution and then ultrasonicated for 10 to 20 minutes at an ultrasonic frequency of 50 to 100 KHz, the oil impurities on the surface of the foam metal conductive substrate can be effectively removed, and the hydrophilicity of the foam metal substrate is improved through the hydroxyl groups in the alcohol solution to obtain a hydrophilic substrate. The alcohol solution used is one or both of ethanol and methanol, and the concentration of the alcohol solution is 99.7%.
[0016] Step 2, loading NiFe-LDH hydrotalcite structure on the surface of hydrophilic substrate:
[0017] A co-precipitation method or a hydrothermal method is adopted to load and form a layer of NiFe-LDH hydrotalcite structure on the surface of the hydrophilic substrate to obtain a modified hydrophilic substrate.
[0018] It should be emphasized that the present invention takes into account that hydrotalcite is an ionic solid containing a layered structure of metal cations with hydroxyl octahedral coordination, and such substances have good stability. Moreover, Ni salts and Fe salts among transition metals are inexpensive and cost-effective, so the present invention preferably uses NiFe-LDH hydrotalcite material as a modified material, and attempts to load a layer of NiFe-LDH hydrotalcite material on the surface of a hydrophilic substrate to increase the material reaction specific surface area and catalytic activity, and obtain a modified hydrophilic substrate.
[0019] It should be noted that when a layer of NiFe-LDH hydrotalcite structure is formed on the surface of the hydrophilic substrate by a hydrothermal method, the hydrophilic substrate is immersed in a NiFe-LDH hydrotalcite precursor solution, and then a hydrothermal reaction is carried out at 120 to 130°C to form a layer of NiFe-LDH hydrotalcite structure on the surface of the hydrophilic substrate to obtain a modified hydrophilic substrate. It can be understood that since NiFe-LDH hydrotalcite needs to be formed, the raw materials for preparing the NiFe-LDH hydrotalcite precursor solution are composed of nickel salt, divalent iron salt, urea and water, wherein the nickel salt and divalent iron salt are used to provide Ni 2+ and Fe 2+Urea is used as a precipitant and decomposes into ammonia and CO3 in the hydrothermal process. 2- , providing alkaline environment and CO3 2- Anions are used for intercalation to form NiFe-LDH layered hydrotalcite. The nickel salt can be any one or more of nickel chloride, nickel nitrate, and nickel sulfate; and the divalent iron salt can be FeCl2 or Fe(NH4)2(SO4)2.
[0020] When a hydrothermal method is used to load and form NiFe-LDH hydrotalcite on the surface of a hydrophilic substrate, each raw material for preparing the NiFe-LDH hydrotalcite material is first formed into a solution, and the formed solution is used as a NiFe-LDH hydrotalcite precursor liquid, and the NiFe-LDH hydrotalcite precursor liquid is subjected to hydrothermal treatment to obtain the NiFe-LDH hydrotalcite material. In order to uniformly load a layer of NiFe-LDH hydrotalcite material on the surface of a hydrophilic substrate, the present invention immerses the hydrophilic substrate in the NiFe-LDH hydrotalcite precursor liquid before the NiFe-LDH hydrotalcite precursor liquid is subjected to hydrothermal treatment, so that the NiFe-LDH hydrotalcite precursor liquid is uniformly dispersed around the hydrophilic substrate, and then during the hydrothermal reaction, the NiFe-LDH hydrotalcite formed by the reaction in the NiFe-LDH hydrotalcite precursor liquid can be uniformly loaded on the surface of the hydrophilic substrate. In order to facilitate the preparation of NiFe-LDH hydrotalcite by hydrothermal synthesis, in a preferred embodiment of the present invention, the usage ratio of nickel salt, divalent iron salt, urea and water used in the present invention is 1.2-6.0 mmol: 0.4-2.0 mmol: 2.0-10.0 mmol: 70 mL.
[0021] It should also be emphasized that in order to ensure that the NiFe-LDH hydrotalcite formed by the reaction in the NiFe-LDH hydrotalcite precursor solution can be uniformly loaded on the surface of the hydrophilic substrate during the hydrothermal reaction, in a preferred embodiment of the present invention, the amount ratio of the hydrophilic carbon cloth to the NiFe-LDH hydrotalcite precursor solution is 9 to 16 cm 2 :70mL.
[0022] In order to ensure that the nickel salt, divalent iron salt and urea in the NiFe-LDH hydrotalcite precursor solution can fully react with each other during the hydrothermal reaction to form NiFe-LDH hydrotalcite on the surface of the hydrophilic substrate, in a preferred embodiment of the present invention, the hydrothermal reaction time is 4 to 24 hours.
[0023] It can be understood that since the system obtained after the hydrothermal reaction is a modified hydrophilic substrate with NiFe-LDH hydrotalcite loaded on the surface, and a solution system, the surface of the modified hydrophilic substrate obtained may have residual unreacted raw materials and solvents, which is not conducive to the subsequent carbon layer coating treatment. Therefore, before the carbon layer coating treatment, the modified hydrophilic substrate obtained after the hydrothermal reaction needs to be washed, and deionized water or distilled water is used as a detergent to wash the surface of the modified hydrophilic substrate, and the washing is performed at least 3 times to remove the residual unreacted raw materials and solvents on its surface, and then the residual water on the surface of the modified hydrophilic substrate is dried to remove the residual water, and then the subsequent step 4 of the carbon layer coating treatment is performed. Among them, the specific method of drying the modified hydrophilic substrate is not limited, as long as the residual water on the surface of the modified hydrophilic substrate can be removed.
[0024] When a layer of NiFe-LDH hydrotalcite structure is formed on the surface of the hydrophilic substrate by coprecipitation method to obtain a modified hydrophilic substrate, it can be understood that since NiFe-LDH hydrotalcite needs to be formed, the mixed salt solution obtained by forming a mixed salt solution with water by nickel salt, divalent iron salt and alkaline solution is mixed to form a NiFe-LDH hydrotalcite precursor solution, and the hydrophilic substrate is immersed in the NiFe-LDH hydrotalcite precursor solution, aged at 80-110°C for 10-24h, washed, and dried to obtain a modified hydrophilic substrate. Among them, the alkaline solution can be selected from any one of ammonia water and sodium carbonate solution to provide an accurate pH environment for the reaction. In order to ensure that the NiFe-LDH hydrotalcite formed by the reaction in the NiFe-LDH hydrotalcite precursor solution during the coprecipitation reaction can be evenly loaded on the surface of the hydrophilic substrate, in a preferred embodiment of the present invention, the amount ratio of nickel salt, divalent iron salt, alkaline solution and water in the NiFe-LDH hydrotalcite precursor solution is 0.3-2.1 mmol: 0.3-0.7 mmol: 16-56 mmol: 30-126 mL.
[0025] Step 3, carbon layer coating pretreatment:
[0026] The modified hydrophilic substrate is immersed in a tris(hydroxymethyl)aminomethane solution, and after being completely immersed, a dopamine hydrochloride solution is added, and after stirring, the substrate is taken out, washed, and dried to form a carbon coating adhesion layer on the surface of the modified hydrophilic substrate to obtain a catalyst precursor.
[0027] It should be noted that the present invention has found in the process of research that if the modified hydrophilic substrate with NiFe-LDH hydrotalcite loaded on the surface is directly used to degrade organic pollutants in sewage, there will be a defect of insufficient oxygen reduction activity and insignificant degradation effect. Therefore, the present invention also performs a carbon layer coating treatment on the basis of the modified hydrophilic substrate.
[0028] It should be emphasized that the present invention takes into account the factor of improving oxygen reduction activity. The modified hydrophilic substrate is first immersed in a tris(hydroxymethyl)aminomethane solution to allow the modified hydrophilic substrate to be fully soaked in the tris(hydroxymethyl)aminomethane solution, and then a dopamine hydrochloride solution is added to allow the tris(hydroxymethyl)aminomethane solution in the reaction system to be fully in contact with the dopamine hydrochloride solution, so that the surface of the modified hydrophilic substrate is fully wrapped by the mixed solution.
[0029] In order to allow the tris(hydroxymethyl)aminomethane solution to fully infiltrate the modified hydrophilic substrate, in a preferred embodiment of the present invention, the amount ratio of the modified hydrophilic substrate to the tris(hydroxymethyl)aminomethane solution is 9 to 16 cm 2 :90mL; wherein the tris(hydroxymethyl)aminomethane solution is prepared by mixing tris(hydroxymethyl)aminomethane and water in a dosage ratio of 0.2 to 0.3 g:90 mL.
[0030] In order to allow the added dopamine hydrochloride solution to fully react with the tris(hydroxymethyl)aminomethane solution, in a preferred embodiment of the present invention, the mass ratio of dopamine hydrochloride in the dopamine hydrochloride solution to tris(hydroxymethyl)aminomethane in the tris(hydroxymethyl)aminomethane solution is 1.8 to 2.2:1.
[0031] In order to make the tris(hydroxymethyl)aminomethane solution fully contact with the dopamine hydrochloride solution to achieve the purpose of uniform solution mixing, in a preferred embodiment of the present invention, when stirring after adding the dopamine hydrochloride solution, the stirring temperature is room temperature, the stirring rate is 50 to 150 r / min, and the stirring time is 4 to 24 hours.
[0032] It is understandable that since unreacted tris(hydroxymethyl)aminomethane solution and dopamine hydrochloride solution may remain on the surface of the catalyst precursor after the stirring treatment, in order to avoid affecting the introduction of impurities other than the carbon layer during the subsequent heating process, the catalyst precursor is taken out from the system after the stirring treatment, and deionized water or distilled water is used as a detergent to wash the surface of the catalyst precursor, and the washing is performed at least 3 times to remove the tris(hydroxymethyl)aminomethane solution and dopamine hydrochloride solution that may remain on its surface, and then the residual water on the surface of the catalyst precursor is dried to remove, and then the subsequent step 4 pyrolysis treatment is performed. Among them, the specific method of drying the catalyst precursor is not limited, as long as the residual water on the surface of the catalyst precursor can be removed.
[0033] Step 4: Pyrolysis treatment to form a carbon layer:
[0034] In a protective gas atmosphere, the catalyst precursor is pyrolyzed at 650-750° C. to transform the carbon-coated adhesion layer into a carbon layer and the NiFe-LDH hydrotalcite structure into a NiFe alloy crystal phase, thereby obtaining the NiFe-based self-supporting electrocatalyst.
[0035] It should be noted that after the above-mentioned dopamine hydrochloride solution and tris (hydroxymethyl) aminomethane solution are jointly processed to the modified hydrophilic substrate, a carbon-coated adhesion layer is formed on the surface of the modified hydrophilic substrate, i.e., a catalyst precursor is obtained. The present invention is subjected to pyrolysis treatment of the catalyst precursor, and the carbon-coated adhesion layer of the modified hydrophilic substrate can be shaped to be converted to form a carbon layer, and during pyrolysis, the carbon-coated adhesion layer on the surface of the catalyst precursor has a trend of thinning, so as to form an ultra-thin carbon layer tightly coated on the substrate surface, and then the catalytic performance of the substrate can be improved. In addition, during high-temperature pyrolysis treatment, NiFe-LDH hydrotalcite can be converted into NiFe alloy crystal phase, and the lamellar structure is maintained at the same time, and the lamellar surface provides ORR active sites, so as to greatly improve the specific surface area and catalytic activity of the substrate material, so that the NiFe-based self-supporting electrocatalyst obtained has high specific surface area and high catalytic activity, so as to obtain a material having a NiFe alloy crystal phase layer and a carbon layer sequentially loaded on the surface, i.e., a NiFe-based self-supporting electrocatalyst.
[0036] In order to ensure that the adhesion layer of dopamine hydrochloride solution and tris(hydroxymethyl)aminomethane solution of the modified hydrophilic substrate can be transformed into a carbon layer, in a preferred embodiment of the present invention, the heating rate of the pyrolysis treatment is 3-7°C / min, the pyrolysis time is 0.5-1.5h, the protective gas used in the pyrolysis treatment is nitrogen or argon, and the flow rate of the protective gas is 20-30mL / min.
[0037] The second object of the present invention is to provide a NiFe-based self-supporting electrocatalyst prepared by the above preparation method.
[0038] The third object of the present invention is to provide an application of the above-mentioned NiFe-based self-supporting electrocatalyst in degrading organic pollutants in sewage.
[0039] Compared with the prior art, the present invention has the following beneficial effects:
[0040] The present invention performs a hydrophilic treatment on a conductive substrate, and then loads a NiFe-LDH hydrotalcite having a unique metal compound sheet array or nanorod array structure on the surface thereof to enhance the specific surface area. Then, an ultra-thin carbon layer is further loaded on the surface of the substrate by coating dopamine hydrochloride and then performing a pyrolysis treatment. Meanwhile, the NiFe-LDH hydrotalcite is transformed into a NiFe alloy crystal phase during the pyrolysis process, and the sheet structure of the hydrotalcite is retained while the NiFe alloy crystal phase is transformed, so that an ORR active site is provided through the sheet surface, thereby greatly improving the specific surface area and catalytic activity of the substrate material, so that the obtained NiFe-based self-supporting electrocatalyst has a high specific surface area and a high catalytic activity to achieve catalyst structure finalization, enhance oxygen reduction activity and catalytic performance, and further obtain a NiFe-based self-supporting electrocatalyst having the structural characteristics of a metal compound sheet array or a nanorod array.
[0041] The preparation process of the present invention is simple, and the electrode preparation cost of the binder and the conductive agent is reduced, while effectively avoiding the disadvantages of difficult recovery of the powder catalyst, low utilization rate, and more electrolytic precipitation in the catalytic process.
[0042] Compared with the traditional electro-Fenton self-supporting electrode, the NiFe-based self-supporting electrocatalyst prepared by the present invention has greatly improved conductivity, high specific surface area and ORR activity. It also has good degradation ability for a variety of organic pollutants, among which Rhodamine B dye can be degraded by more than 98% in 1 hour. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is a scanning electron microscope image of the NiFe-based self-supporting electrocatalyst prepared in Example 1 at a scale of 1 μm.
[0044] Figure 2 This is a scanning electron microscope image of the NiFe-based self-supporting electrocatalyst prepared in Example 1 at a scale of 500 nm.
[0045] Figure 3 This is the XRD pattern of the NiFe-based self-supporting electrocatalyst prepared in Example 1.
[0046] Figure 4 This is the CV curve of the NiFe-based self-supporting electrocatalyst prepared in Example 1.
[0047] Figure 5 This is a degradation effect curve diagram of the NiFe-based self-supporting electrocatalyst prepared in Example 1 for degrading tetracycline hydrochloride, oxytetracycline hydrochloride, and rhodamine B. DETAILED DESCRIPTION
[0048] The technical solutions in the embodiments of the present invention will be described clearly and completely below.
[0049] Example 1
[0050] This embodiment provides a NiFe-based self-supporting electrocatalyst, and the preparation method thereof comprises the following steps:
[0051] Step 1, hydrophilization treatment:
[0052] 1) Cut the commercially available carbon cloth into a size of 3 cm×4 cm, then completely immerse it in 50 mL of ethanol, and then place it in a water bath at 85° C. and heat it to boil for 20 min to remove the surface hydrophobic coating to obtain a clean carbon cloth.
[0053] 2) The cleaned carbon cloth was immersed in 30 mL of 3 mol / L hydrochloric acid, and ultrasonicated for 30 min at an ultrasonic frequency of 60 kHz to remove impurities. Then, deionized water was used as a detergent to wash the surface of the carbon cloth until the pH of the washing liquid was neutral, and then dried in an oven at 60°C to obtain a hydrophilic substrate.
[0054] Step 2: Using a hydrothermal method, a layer of NiFe-LDH hydrotalcite structure is loaded on the surface of a hydrophilic substrate:
[0055] 1) Preparation of NiFe-LDH hydrotalcite precursor solution:
[0056] 0.6 mmol FeCl2·4H2O, 1.8 mmol NiCl2·6H2O, and 3.0 mmol CO(NH2)2 were dissolved in 70 mL of deionized water and stirred thoroughly to form a transparent solution to obtain a NiFe-LDH hydrotalcite precursor solution.
[0057] 2) Hydrothermal reaction:
[0058] The NiFe-LDH hydrotalcite precursor solution obtained above was placed in a reactor with 100 mL of polytetrafluoroethylene as the substrate, and then the hydrophilic substrate obtained above was immersed in the NiFe-LDH hydrotalcite precursor solution in the reactor, and then placed in an oven at 125°C for hydrothermal reaction for 6.5 hours. After the reaction was completed, the hydrophilic substrate was taken out, and distilled water was used as a detergent to wash the surface of the hydrophilic substrate for 3 times to remove the raw materials and solvents that may have remained on the surface and not reacted completely, and then placed in an oven at 80°C for drying to remove the residual water on the surface of the carbon cloth, and obtain a modified hydrophilic substrate.
[0059] Step 3, carbon layer coating pretreatment:
[0060] 1) Dissolve 0.25 g of tris(hydroxymethyl)aminomethane in 90 mL of distilled water to obtain a tris(hydroxymethyl)aminomethane solution.
[0061] 2) Dissolve 500 mg of dopamine hydrochloride in 90 mL of distilled water to obtain a dopamine hydrochloride solution.
[0062] 3) The modified hydrophilic substrate obtained above is immersed in the tris(hydroxymethyl)aminomethane solution obtained above, and after complete immersion, the prepared dopamine hydrochloride solution is added, and stirred at room temperature at a stirring rate of 100 r / min for 6 hours. The substrate is removed, and the surface of the substrate is washed 3 times with distilled water as a detergent, and then placed in an oven at 80°C to dry, and the residual water on the surface of the carbon cloth is dried to obtain a catalyst precursor.
[0063] Step 4: Pyrolysis treatment to form a carbon layer:
[0064] Under a flowing nitrogen atmosphere, the catalyst precursor obtained in the above step was placed in a tubular furnace, the heating rate was set to 5°C / min, and the temperature was kept at 700°C for 1 h. The nitrogen flow rate was 25 mL / min to obtain a NiFe-based self-supporting electrocatalyst.
[0065] Example 2
[0066] This embodiment provides a NiFe-based self-supporting electrocatalyst, and the preparation method thereof comprises the following steps:
[0067] Step 1, hydrophilization treatment:
[0068] The commercially available nickel foam was cut into a size of 3 cm×4 cm, and then completely immersed in 50 mL of ethanol and ultrasonicated for 15 min at an ultrasonic frequency of 60 KHz to obtain a clean nickel foam.
[0069] Step 2: Using a hydrothermal method, a layer of NiFe-LDH hydrotalcite structure is loaded on the surface of a hydrophilic substrate:
[0070] 1) Preparation of NiFe-LDH hydrotalcite precursor solution:
[0071] 0.6 mmol FeCl2·4H2O, 1.8 mmol NiCl2·6H2O, and 3.0 mmol CO(NH2)2 were dissolved in 70 mL of deionized water and stirred thoroughly to form a transparent solution to obtain a NiFe-LDH hydrotalcite precursor solution.
[0072] 2) Hydrothermal reaction:
[0073] The NiFe-LDH hydrotalcite precursor solution obtained above was placed in a reactor with 100 mL of polytetrafluoroethylene as the substrate, and then the hydrophilic substrate obtained above was immersed in the NiFe-LDH hydrotalcite precursor solution in the reactor, and then placed in an oven at 125°C for hydrothermal reaction for 6.5 hours. After the reaction was completed, the hydrophilic substrate was taken out, and distilled water was used as a detergent to wash the surface of the hydrophilic substrate for 3 times to remove the raw materials and solvents that may have remained on the surface and not reacted completely, and then placed in an oven at 80°C for drying to remove the residual water on the surface of the carbon cloth, and obtain a modified hydrophilic substrate.
[0074] Step 3, carbon layer coating pretreatment:
[0075] 1) Dissolve 0.25 g of tris(hydroxymethyl)aminomethane in 90 mL of distilled water to obtain a tris(hydroxymethyl)aminomethane solution.
[0076] 2) Dissolve 550 mg of dopamine hydrochloride in 90 mL of distilled water to obtain a dopamine hydrochloride solution.
[0077] 3) The modified hydrophilic substrate obtained above is immersed in the tris(hydroxymethyl)aminomethane solution obtained above, and after complete immersion, the prepared dopamine hydrochloride solution is added, and stirred at room temperature at a stirring rate of 100 r / min for 24 hours. The substrate is removed, and the surface of the substrate is washed three times with distilled water as a detergent, and then placed in an oven at 80°C to dry, and the residual water on the surface of the carbon cloth is dried to obtain a catalyst precursor.
[0078] Step 4: Pyrolysis treatment to form a carbon layer:
[0079] Under a flowing nitrogen atmosphere, the catalyst precursor obtained in the above step was placed in a tubular furnace, the heating rate was set to 5°C / min, and the temperature was kept at 700°C for 1 h. The nitrogen flow rate was 25 mL / min to obtain a NiFe-based self-supporting electrocatalyst.
[0080] That is, the difference between this embodiment and embodiment 1 is only that:
[0081] The substrate used in this embodiment is nickel foam; and in step 4, the stirring time after adding the dopamine hydrochloride solution is 24 hours.
[0082] The catalytic performance of the catalyst was tested, and the degradation rate of Rhodamine B pollutant in 1 hour was about 80%.
[0083] Example 3
[0084] This embodiment provides a NiFe-based self-supporting electrocatalyst, and the preparation method thereof comprises the following steps:
[0085] Step 1, hydrophilization treatment:
[0086] 1) Cut the commercially available carbon cloth into a size of 3 cm×3 cm, then completely immerse it in 50 mL of ethanol, and then heat and boil it in a water bath at 82° C. for 15 min to remove the surface hydrophobic coating to obtain a clean carbon cloth.
[0087] 2) The cleaned carbon cloth was immersed in 30 mL of 2.5 mol / L hydrochloric acid, and ultrasonicated for 20 min at an ultrasonic frequency of 50 kHz to remove impurities. Then, deionized water was used as a detergent to wash the surface of the carbon cloth until the pH of the washing liquid was neutral, and then dried in an oven at 60°C to obtain a hydrophilic substrate.
[0088] Step 2: Using a hydrothermal method, a layer of NiFe-LDH hydrotalcite structure is loaded on the surface of a hydrophilic substrate:
[0089] 1) Preparation of NiFe-LDH hydrotalcite precursor solution:
[0090] 0.6 mmol FeCl2·4H2O, 1.8 mmol NiCl2·6H2O, and 3.0 mmol CO(NH2)2 were dissolved in 70 mL of deionized water and stirred thoroughly to form a transparent solution to obtain a NiFe-LDH hydrotalcite precursor solution.
[0091] 2) Hydrothermal reaction:
[0092] The NiFe-LDH hydrotalcite precursor solution obtained above was placed in a reactor with 100 mL of polytetrafluoroethylene as the substrate, and then the hydrophilic substrate obtained above was immersed in the NiFe-LDH hydrotalcite precursor solution in the reactor, and then placed in an oven at 120°C for hydrothermal reaction for 8 hours. After the reaction was completed, the hydrophilic substrate was taken out, and distilled water was used as a detergent to wash the surface of the hydrophilic substrate for 3 times to remove the raw materials and solvents that may have remained on the surface and not reacted completely, and then placed in an oven at 80°C for drying to remove the residual water on the surface of the carbon cloth, and obtain a modified hydrophilic substrate.
[0093] Step 3, carbon layer coating pretreatment:
[0094] 1) Dissolve 0.2 g of tris(hydroxymethyl)aminomethane in 90 mL of distilled water to obtain a tris(hydroxymethyl)aminomethane solution.
[0095] 2) Dissolve 360 mg of dopamine hydrochloride in 90 mL of distilled water to obtain a dopamine hydrochloride solution.
[0096] 3) The modified hydrophilic substrate obtained above is immersed in the tris(hydroxymethyl)aminomethane solution obtained above, and after complete immersion, the prepared dopamine hydrochloride solution is added, and stirred at room temperature at a stirring rate of 100 r / min for 4 hours. The substrate is removed, and the surface of the substrate is washed 3 times with distilled water as a detergent, and then placed in an oven at 80°C to dry, and the residual water on the surface of the carbon cloth is dried to obtain a catalyst precursor.
[0097] Step 4: Pyrolysis treatment to form a carbon layer:
[0098] Under a flowing nitrogen atmosphere, the catalyst precursor obtained in the above step was placed in a tubular furnace, the heating rate was set to 3°C / min, and the temperature was kept at 600°C for 0.5h. The nitrogen flow rate was 20mL / min to obtain a NiFe-based self-supporting electrocatalyst.
[0099] Example 4
[0100] This embodiment provides a NiFe-based self-supporting electrocatalyst, and the preparation method thereof comprises the following steps:
[0101] Step 1, hydrophilization treatment:
[0102] 1) Cut the commercially available carbon cloth into a size of 4 cm×4 cm, then completely immerse it in 50 mL of ethanol, and then heat and boil it in a water bath at 88° C. for 25 min to remove the surface hydrophobic coating to obtain a clean carbon cloth.
[0103] 2) The cleaned carbon cloth is immersed in 30 mL of 3.5 mol / L hydrochloric acid, and ultrasonically treated for 30 min under ultrasonic conditions with an ultrasonic power or ultrasonic frequency of 60 kHz to remove impurities. Then, distilled water is used as a detergent to wash the surface of the carbon cloth until the pH of the washing liquid is neutral, and then the carbon cloth is dried in an oven at 60°C to obtain a hydrophilic substrate.
[0104] Step 2: Using a hydrothermal method, a layer of NiFe-LDH hydrotalcite structure is loaded on the surface of a hydrophilic substrate:
[0105] 1) Preparation of NiFe-LDH hydrotalcite precursor solution:
[0106] 6 mmol FeCl2·4H2O, 2.0 mmol NiCl2·6H2O, and 10.0 mmol CO(NH2)2 were dissolved in 70 mL deionized water and stirred thoroughly to form a transparent solution to obtain a NiFe-LDH hydrotalcite precursor solution.
[0107] 2) Hydrothermal reaction:
[0108] The NiFe-LDH hydrotalcite precursor solution obtained above was placed in a reactor with 100 mL of polytetrafluoroethylene as the substrate, and then the hydrophilic substrate obtained above was immersed in the NiFe-LDH hydrotalcite precursor solution in the reactor, and then placed in an oven at 130°C for hydrothermal reaction for 8 hours. After the reaction was completed, the hydrophilic substrate was taken out, and distilled water was used as a detergent to wash the surface of the hydrophilic substrate for 3 times to remove the raw materials and solvents that may have remained on the surface and not reacted completely, and then placed in an oven at 80°C for drying to remove the residual water on the surface of the carbon cloth, and obtain a modified hydrophilic substrate.
[0109] Step 3, carbon layer coating pretreatment:
[0110] 1) Dissolve 0.3 g of tris(hydroxymethyl)aminomethane in 90 mL of distilled water to obtain a tris(hydroxymethyl)aminomethane solution.
[0111] 2) Dissolve 660 mg of dopamine hydrochloride in 90 mL of distilled water to obtain a dopamine hydrochloride solution.
[0112] 3) The modified hydrophilic substrate obtained above is immersed in the tris(hydroxymethyl)aminomethane solution obtained above, and after complete immersion, the prepared dopamine hydrochloride solution is added, and stirred at room temperature at a stirring rate of 100 r / min for 12 hours. The substrate is removed, and the surface of the substrate is washed three times with distilled water as a detergent, and then placed in an oven at 80°C for drying to remove the residual water on the surface of the carbon cloth to obtain a catalyst precursor.
[0113] Step 4: Pyrolysis treatment to form a carbon layer:
[0114] Under a flowing nitrogen atmosphere, the catalyst precursor obtained in the above step was placed in a tubular furnace, the heating rate was set to 7°C / min, and the temperature was kept at 800°C for 1 h. The nitrogen flow rate was 30 mL / min to obtain a NiFe-based self-supporting electrocatalyst.
[0115] Example 5
[0116] This embodiment provides a NiFe-based self-supporting electrocatalyst, and the preparation method thereof comprises the following steps:
[0117] Step 1, hydrophilization treatment:
[0118] 1) Cut the commercially available carbon cloth into a size of 3 cm×4 cm, then completely immerse it in 50 mL of ethanol, and then place it in a water bath at 85° C. and heat it to boil for 20 min to remove the surface hydrophobic coating to obtain a clean carbon cloth.
[0119] 2) The cleaned carbon cloth was immersed in 30 mL of 3 mol / L hydrochloric acid, and ultrasonicated for 30 min at an ultrasonic frequency of 60 kHz to remove impurities. Then, distilled water was used as a detergent to wash the surface of the carbon cloth until the pH of the washing liquid was neutral, and then dried in an oven at 60°C to obtain a hydrophilic substrate.
[0120] Step 2: Using the co-precipitation method, a layer of NiFe-LDH hydrotalcite structure is loaded on the surface of the hydrophilic substrate:
[0121] 1) Preparation of NiFe-LDH hydrotalcite precursor solution:
[0122] Dissolve 0.6mmol FeCl2·4H2O and 1.8mmol NiCl2·6H2O in 50mL deionized water and stir thoroughly to form a transparent solution to obtain mixed solution A. Dissolve 40mmol sodium carbonate in 40mL deionized water to obtain a sodium carbonate solution. Pour the uniformly mixed sodium carbonate solution into solution A at room temperature and stir thoroughly to finally prepare a NiFe-LDH hydrotalcite precursor solution.
[0123] 2) Aging reaction:
[0124] The hydrophilic substrate obtained in step 1 above was immersed in the NiFe-LDH hydrotalcite precursor solution and aged at 100°C for 20h. After the reaction was completed, the hydrophilic substrate was taken out, and the surface of the hydrophilic substrate was washed with distilled water as a detergent for 3 times to remove the raw materials and solvents that may have remained on the surface and not reacted completely, and then placed in an oven at 80°C to dry and remove the residual water on the surface of the carbon cloth to obtain a modified hydrophilic substrate.
[0125] Step 3, carbon layer coating pretreatment:
[0126] 1) Dissolve 0.25 g of tris(hydroxymethyl)aminomethane in 90 mL of distilled water to obtain a tris(hydroxymethyl)aminomethane solution.
[0127] 2) Dissolve 500 mg of dopamine hydrochloride in 90 mL of distilled water to obtain a dopamine hydrochloride solution.
[0128] 3) The modified hydrophilic substrate obtained above is immersed in the tris(hydroxymethyl)aminomethane solution obtained above, and after complete immersion, the prepared dopamine hydrochloride solution is added, and stirred at room temperature at a stirring rate of 100 r / min for 6 hours. The substrate is removed, and the surface of the substrate is washed 3 times with distilled water as a detergent, and then placed in an oven at 80°C to dry, and the residual water on the surface of the carbon cloth is dried to obtain a catalyst precursor.
[0129] Step 4: Pyrolysis treatment to form a carbon layer:
[0130] Under a flowing nitrogen atmosphere, the catalyst precursor obtained in the above step was placed in a tubular furnace, the heating rate was set to 5°C / min, and the temperature was kept at 700°C for 1 h. The nitrogen flow rate was 25 mL / min to obtain a NiFe-based self-supporting electrocatalyst.
[0131] Comparative Example 1
[0132] This comparative example provides a NiFe-based self-supporting electrocatalyst, and its preparation method comprises the following steps:
[0133] Step 1, hydrophilization treatment:
[0134] 1) Cut the commercially available carbon cloth into a size of 3 cm×4 cm, then completely immerse it in 50 mL of ethanol, and then place it in a water bath at 85° C. and heat it to boil for 20 min to remove the surface hydrophobic coating to obtain a clean carbon cloth.
[0135] 2) The cleaned carbon cloth is immersed in 30 mL of 3 mol / L hydrochloric acid, and ultrasonically treated for 30 min under ultrasonic conditions with an ultrasonic power or ultrasonic frequency of 60 kHz to remove impurities. Then, distilled water is used as a detergent to wash the surface of the carbon cloth until the pH of the washing liquid is neutral, and then the carbon cloth is dried in an oven at 60°C to obtain a hydrophilic substrate.
[0136] Step 2, prepare NiFe-LDH hydrotalcite precursor solution:
[0137] 0.6 mmol FeCl2·4H2O, 1.8 mmol NiCl2·6H2O, and 3.0 mmol CO(NH2)2 were dissolved in 70 mL of deionized water and stirred thoroughly to form a transparent solution to obtain a NiFe-LDH hydrotalcite precursor solution.
[0138] Step 3, hydrothermal reaction:
[0139] The NiFe-LDH hydrotalcite precursor solution obtained above was placed in a reactor with 100 mL of polytetrafluoroethylene as the substrate, and then the hydrophilic substrate obtained above was immersed in the NiFe-LDH hydrotalcite precursor solution in the reactor, and then placed in an oven at 120°C for hydrothermal reaction for 6 hours. After the reaction was completed, the hydrophilic substrate was taken out, and distilled water was used as a detergent to wash the surface of the hydrophilic substrate for 3 times to remove the raw materials and solvents that may have remained on the surface and not reacted completely, and then placed in an oven at 80°C for drying to remove the residual water on the surface of the carbon cloth, and the obtained product was used as a NiFe-based self-supporting electrocatalyst.
[0140] That is, the difference between this comparative example and Example 1 is only that:
[0141] The carbon layer coating pretreatment and pyrolysis treatment of steps 4 and 5 were not carried out.
[0142] Experimental Section
[0143] (I) Morphology Test
[0144] Taking the NiFe-based self-supported electrocatalyst prepared in Example 1 of the present invention as an example, it was subjected to scanning electron microscopy (SEM) test, and the test results are as Figure 1 and Figure 2 shown. Among them, Figure 1 is the SEM image of the NiFe-based self-supported electrocatalyst prepared in Example 1 at a scale of 1 μm, Figure 2 is the SEM image of the NiFe-based self-supported electrocatalyst prepared in Example 1 at a scale of 500 nm.
[0145] From Figure 1 and Figure 2 the test results, it can be seen that the NiFe-based self-supported electrocatalyst prepared in Example 1 is covered with a layer of array-like metal compounds, which indicates that the preparation method of the present invention can successfully grow a dense layer of NiFe substance on the three-dimensional structure of the hydrophilic carbon cloth. And a structure similar to nanosheets can be observed in this catalyst, proving that the carbon layer has been wrapped on the nickel-iron hydrotalcite.
[0146] (II) XRD Test
[0147] Taking the NiFe-based self-supported electrocatalyst prepared in Example 1 of the present invention as an example, it was subjected to XRD test, and the test results are as Figure 3 shown. Figure 3 In
[0148] From Figure 3 the test results, it can be seen that the XRD characteristic peaks of the FeNi-based self-supported catalyst correspond to the standard card of the FeNi (PDF#47-1417) alloy phase, proving that the NiFe hydrotalcite is transformed into FeNi alloy after pyrolysis. In addition, a sharp carbon crystallization peak appears at about 26°, indicating that the carbon layer is successfully coated on the surface of the NiFe alloy.
[0149] (III) Electrochemical Performance Test
[0150] Taking the NiFe-based self-supported electrocatalyst prepared in Example 1 of the present invention as an example, cyclic voltammetry tests were carried out on it in 0.05 mol / L Na2SO4 solution without O2 and O2-saturated, and the test results are as Figure 4 shown. Figure 4In the figure, the Chinese name corresponding to the English word "Potential" on the horizontal axis is "voltage", which indicates the voltage value applied by the electrode; the Chinese name corresponding to the English word "Currentdensity" on the vertical axis is "current density"; and "O2free" indicates the cyclic voltammetry test results under the condition of no O2, and "O2" indicates the cyclic voltammetry test results under the condition of O2 saturation.
[0151] Depend on Figure 4 The test results show that the NiFe-based self-supporting catalyst prepared in Example 1 is Figure 4 In the potential range of -0.1 to 1.1 V, there is no obvious oxygen reduction peak. However, under the condition of O2 saturation, the NiFe-based self-supporting catalyst prepared in Example 1 has an obvious oxygen reduction peak at about 0.42 V, indicating that the NiFe-based self-supporting catalyst prepared in Example 1 has good oxygen reduction activity.
[0152] The present invention also takes the NiFe-based self-supporting electrocatalyst prepared in Comparative Example 1 as an example, and conducts a cyclic voltammetry test on it in an O2-saturated 0.05 mol / LNa2SO4 solution. The test results show that no obvious oxygen reduction peak is observed when Comparative Example 1 is tested under O2-saturated conditions, which also indicates that the oxygen reduction effect and degradation performance of Comparative Example 1 are not as good as those of the NiFe-based self-supporting electrocatalyst.
[0153] Based on the above, it can be seen that the carbon layer pre-coating treatment and the pyrolysis treatment play an important role in forming the carbon layer and transforming the NiFe-LDH hydrotalcite into NiFe alloy crystals to improve the electrochemical properties of the substrate.
[0154] (IV) Degradation effect test
[0155] The present invention adds 2 cm×2 cm of the NiFe-based self-supporting electrocatalyst of Example 1 as a degradation material to 90 mL of an electrolyte solution containing 10 mg / L tetracycline hydrochloride, 90 mL of an electrolyte solution containing 10 mg / L oxytetracycline hydrochloride, and 90 mL of an electrolyte solution containing 10 mg / L rhodamine B, respectively, and tests the degradation efficiency of the organic pollutants. The test results are as follows: Figure 5 The degradation efficiency is shown in To evaluate, where C represents the concentration after degradation and C0 represents the initial concentration of organic pollutants.
[0156] Depend on Figure 5It can be seen from the test results that the NiFe-based self-supporting electrocatalyst prepared in Example 1 can effectively degrade pollutants such as tetracycline hydrochloride, oxytetracycline hydrochloride and rhodamine B. Among them, within 70 minutes, the degradation efficiency of the NiFe-based self-supporting electrocatalyst prepared in Example 1 for oxytetracycline hydrochloride in a 10 mg / L oxytetracycline hydrochloride aqueous solution reached more than 70%. Within 70 minutes, the degradation efficiency of the NiFe-based self-supporting electrocatalyst prepared in Example 1 for tetracycline hydrochloride in a 10 mg / L tetracycline hydrochloride aqueous solution reached more than 60%. And within 60 minutes, the degradation efficiency of the NiFe-based self-supporting electrocatalyst prepared in Example 1 for rhodamine B in a 10 mg / L rhodamine B aqueous solution reached more than 98%, and the degradation effect was significant.
[0157] The present invention also uses Example 2 as a degradation agent, and takes a 2cm×2cm NiFe-based self-supporting electrocatalyst prepared in Example 2 and places it in a 90mL Rhodamine B aqueous solution containing 10mg / L Rhodamine B for catalytic performance testing. And the test results show that within 60min, the degradation rate of Rhodamine B in a 10mg / L Rhodamine B aqueous solution by the NiFe-based self-supporting electrocatalyst prepared in Example 2 is about 80%. And from the above test results, it can be seen that within 60min, the degradation efficiency of Rhodamine B in a 10mg / L Rhodamine B aqueous solution by the NiFe-based self-supporting electrocatalyst prepared in Example 1 reaches more than 98%, which shows that the choice of substrate has a greater influence on the loading effect of the carbon layer. Compared with nickel foam, carbon cloth is more conducive to loading NiFe-LDH hydrotalcite and carbon layer, thereby having a higher specific surface area and catalytic activity.
[0158] It should be noted that the test method for the above-mentioned degradation effect test of the present invention is as follows:
[0159] The degradation performance test was carried out on an electrochemical workstation (CHI760E). Na2SO4, FeSO4·7H2O, the above-mentioned organic pollutants to be degraded and distilled water were prepared to form a mixed solution containing 0.05 mol / L Na2SO4, 10 mg / L organic pollutants to be degraded, and a pH of 3 (the pH of the solution was adjusted to 3 using sulfuric acid). The mixed solution was used as an electrolyte solution, and a three-electrode system was used. In the above-mentioned electrolyte solution, a NiFe-based self-supporting electrocatalyst was used as a working electrode, a mercury / mercury oxide electrode was used as a reference electrode, and a platinum electrode was used as a counter electrode for testing.
[0160] Obviously, the above embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
Claims
1. A method for preparing a NiFe-based self-supporting electrocatalyst, characterized in that: The following steps are involved: Performing hydrophilization treatment on the conductive substrate to obtain a hydrophilic substrate; A layer of NiFe-LDH hydrotalcite structure is loaded on the surface of the hydrophilic substrate by a co-precipitation method or a hydrothermal method to obtain a modified hydrophilic substrate; After immersing the modified hydrophilic substrate in a tris(hydroxymethyl)aminomethane solution, adding a dopamine hydrochloride solution and stirring the solution to form a carbon coating adhesion layer on the surface of the modified hydrophilic substrate to obtain a catalyst precursor; In a protective gas atmosphere, the catalyst precursor is pyrolyzed at 650-750° C. to transform the carbon-coated adhesion layer into a carbon layer and the NiFe-LDH hydrotalcite structure into a NiFe alloy crystal phase, thereby obtaining the NiFe-based self-supporting electrocatalyst; The amount ratio of the modified hydrophilic substrate to the tris(hydroxymethyl)aminomethane solution is 9 to 16 cm 2 :90mL; The tris(hydroxymethyl)aminomethane solution is prepared by mixing tris(hydroxymethyl)aminomethane and water in a dosage ratio of 0.2-0.3 g:90 mL; The mass ratio of dopamine hydrochloride in the dopamine hydrochloride solution to tris(hydroxymethyl)aminomethane in the tris(hydroxymethyl)aminomethane solution is 1.8-2.2:1; The conductive substrate is foam metal or carbon fiber material; The hydrophilization treatment is achieved by the following steps: When the carbon fiber material is used as the conductive substrate, an alcohol solution is used as a pretreatment agent, the conductive substrate is fully soaked in the alcohol solution, and then boiled at 82 to 88° C. and continuously boiled for 15 to 25 minutes to remove the hydrophobic coating on the surface of the conductive substrate, thereby obtaining a pretreated conductive substrate; Then, using acid solution as a treating agent, subjecting the pretreated conductive substrate to ultrasonic treatment in the acid solution to improve the hydrophilicity of the pretreated conductive substrate, thereby obtaining the hydrophilic substrate; When foamed metal is used as the conductive substrate, an alcohol solution is used as the treatment solution, and the conductive substrate is ultrasonically treated in the alcohol solution to remove impurities on the surface of the foamed metal conductive substrate and to improve the hydrophilicity of the foamed metal substrate through the hydroxyl groups in the alcohol solution, thereby obtaining the hydrophilic substrate.
2. The preparation method according to claim 1, characterized in that The alcohol solution is one or both of ethanol and methanol, and the concentration of the alcohol solution is 99.7%.
3. The preparation method according to claim 1, characterized in that: The ratio of the conductive substrate to the acid solution is 9 to 16 cm 2 :30mL; and the concentration of the acid solution is 2.5~3.5mol / L.
4. The preparation method according to claim 1, characterized in that: The pyrolysis time of the pyrolysis treatment is 0.5 to 1.5 hours.
5. A NiFe-based self-supporting electrocatalyst prepared by the preparation method according to any one of claims 1 to 4.
6. Use of the NiFe-based self-supporting electrocatalyst according to claim 5 for degrading organic pollutants in sewage.
Citation Information
Patent Citations
Carbon-coated nickel-iron alloy nanocatalyst as well as preparation method and application of carbon-coated nickel-iron alloy nanocatalyst
CN108579760A
FeNi / N-C high-dispersion core-shell structure catalyst and preparation method thereof
CN108906106A
Transition metal nanoparticle catalyst coated with graphitized carbon layer and preparation method of transition metal nanoparticle catalyst
CN113410475A
Preparation method of modified ferro-nickel layered double hydroxide composite nano photocatalyst
CN114029044A
Foamed nickel supported nickel-iron bimetallic oxyhydroxide composite catalyst as well as preparation method and application thereof
CN114643057A