A scale-inhibiting and dispersing corrosion inhibitor and its preparation method and application

By copolymerizing starch with maleic anhydride and hydrogen peroxide, a copolymer with excellent scale inhibition, dispersion and corrosion inhibition properties is prepared, which solves the problem of eutrophication of water bodies caused by existing water treatment agents and realizes environmentally friendly, low-cost industrial recycling water. deal with.

CN118126246BActive Publication Date: 2024-10-22ENERGY RESOURCES INST HEBEI ACADEMY OF SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410572691.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2024-10-22
Estimated Expiration
2044-05-10

AI Technical Summary

Technical Problem

The water treatment agents in existing industrial circulating cooling water systems contain phosphorus or nitrogen. Long-term use can easily lead to eutrophication of the water body. The application of oxidized starch in copolymers has not yet been reported, and the performance of scale and dispersion inhibitors is insufficient.

Method used

Maleic anhydride and hydrogen peroxide oxidized starch are copolymerized with a mass ratio of 2 to 5:1. By stirring in distilled water, heating and gelatinizing, and adding ceric ammonium nitrate solution for dropwise addition and polymerization, a product with excellent scale inhibition, dispersion and slowing down is prepared. Corrosion-resistant copolymers.

Benefits of technology

Significantly improved scale inhibition performance, dispersion performance and corrosion inhibition performance, low cost, environmentally friendly monomer selection, green synthesis process, no pollution, suitable for industrial recycling water treatment, reducing treatment costs, does not contain phosphorus and nitrogen elements, and is friendly to the water environment .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

The present invention relates to a scale-inhibiting and dispersing corrosion inhibitor, a preparation method and application thereof, which is obtained by copolymerizing maleic anhydride and hydrogen peroxide oxidized starch, wherein the mass ratio of the maleic anhydride to the hydrogen peroxide oxidized starch is 2 to 5: 1. The polymer provided by the present invention has excellent scale-inhibiting performance, iron oxide dispersing and corrosion-inhibiting performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water treatment, and in particular to a scale-inhibiting and dispersing corrosion inhibitor and a preparation method and application thereof. Background Art

[0002] At present, most of the chemicals used in industrial circulating cooling water systems contain phosphorus or nitrogen, which can easily lead to eutrophication of water bodies and are not environmentally friendly if used for a long time. The applicant has carried out a lot of research work to improve the performance and environmental friendliness of water treatment agents in industrial circulating cooling water systems.

[0003] The use of oxidized starch in water treatment scale inhibitors has been reported, but it appears in the form of a uniform composition, mixed with other ingredients for water treatment. For example, CN102452723A discloses a phosphorus-free composite scale inhibitor, which is made by mixing 10% to 13% polyaspartic acid, 25% to 28% sodium lignin sulfate, 10% to 13% oxidized starch, and 50% to 55% deionized water. CN110342654A discloses a new type of phosphorus-free corrosion inhibitor, characterized in that it is made of the following raw materials in mass percentage: 30-80% of a modified chitosan quaternary ammonium salt mixture, 10-50% of an oxidized starch mixture, and 10-25% of an alkylamine emulsion.

[0004] There are no reports on oxidized starch in copolymers. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects in the prior art, provide a scale-inhibiting and dispersing corrosion inhibitor, and also provide a preparation method and application thereof.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] On one hand, the present invention provides a scale-dispersing corrosion inhibitor, which is obtained by copolymerizing maleic anhydride and hydrogen peroxide oxidized starch, wherein the mass ratio of the maleic anhydride to the hydrogen peroxide oxidized starch is 2-5:1.

[0008] As some preferred embodiments of the present invention, the mass ratio of the maleic anhydride to the hydrogen peroxide oxidized starch is 4:1.

[0009] As some preferred embodiments of the present invention, it comprises the following steps:

[0010] Add hydrogen peroxide oxidized starch into distilled water and stir until it is in a suspension state. Pass nitrogen and heat to 75-85°C for gelatinization for 0.5-1h. Add ammonium cerium nitrate solution and stir for a while. Add maleic anhydride solution dropwise and polymerize at a constant temperature for 5-6h after the addition is completed. After the polymerization is completed, dry the product to obtain the product.

[0011] As some preferred embodiments of the present invention, the amount of the ammonium cerium nitrate added is 2-4% of the total mass of maleic anhydride and the hydrogen peroxide oxidized starch; the mass concentration of the ammonium cerium nitrate solution is 0.4-0.6%.

[0012] As some preferred embodiments of the present invention, hydrogen peroxide oxidized starch is added to 10 to 15 times the mass of distilled water and stirred for dispersion, and the mass percentage of the maleic anhydride aqueous solution is 10 to 20%.

[0013] As some preferred embodiments of the present invention, the ammonium cerium nitrate solution is added and stirred for 15 to 30 minutes, and the maleic anhydride is added dropwise for 0.5 to 1 hour.

[0014] As some preferred embodiments of the present invention, the oxidized starch is prepared as follows:

[0015] Add distilled water to soluble corn starch and stir until it becomes a paste. Use sodium hydroxide solution to adjust the pH value to 5-7. Heat to 40-60°C, slowly add 30% hydrogen peroxide, react for 3-5 hours, filter the obtained solution, wash with distilled water, and dry to obtain hydrogen peroxide oxidized starch solid.

[0016] As some preferred embodiments of the present invention, the amount of the 30% hydrogen peroxide added is 20% of the mass of the soluble starch.

[0017] As some preferred embodiments of the present invention, the mass ratio of the soluble corn starch to distilled water is 1:10.

[0018] Another aspect of the present invention provides the use of the above-mentioned scale inhibitor, dispersant and slow-release agent as a water treatment agent in industrial circulating cooling water.

[0019] The beneficial effects of adopting the above technical solution are:

[0020] 1. The polymer provided by the present invention has excellent scale inhibition performance, iron oxide dispersion and corrosion inhibition performance.

[0021] 2. The polymer provided by the present invention has significantly improved scale inhibition, dispersibility and corrosion inhibition performance through monomer selection and ratio adjustment, and has a synergistic effect.

[0022] 3. The polymer provided by the present invention is low in cost, the initiator greatly promotes the polymerization of the monomer, and the preparation method has a high degree of polymerization, which can greatly reduce industrial costs and reduce the treatment cost of industrial circulating water.

[0023] 4. The monomers used and the synthesized copolymers do not contain phosphorus and nitrogen elements that may cause eutrophication of water bodies, and their application is friendly to the water environment and does not pollute the water body.

[0024] 5. The monomers used in the polymer are all environmentally friendly compounds, and the synthesis process is green and pollution-free, and the obtained product is an environmentally friendly green agent. DETAILED DESCRIPTION

[0025] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention is clearly and completely described below in conjunction with specific embodiments.

[0026] Preparation Example 1

[0027] A certain amount of soluble corn starch and distilled water equivalent to 10 times its mass were added to a four-necked flask and stirred until it became a paste. The pH value was adjusted to 6 with a sodium hydroxide solution with a mass concentration of 1%, and the water bath was heated to 50°C. 30% hydrogen peroxide was slowly added to the system by a syringe pump (the amount of hydrogen peroxide added was 20% of the mass of starch). The pH value was kept constant during this process. After the addition was completed, the solution in the system reacted for 4 hours, and the obtained solution was filtered, washed with distilled water and dried to finally obtain hydrogen peroxide oxidized starch (OS) solid.

[0028] Preparation Example 2

[0029] A certain amount of soluble corn starch and distilled water equivalent to 10 times its mass were added to a four-necked flask and stirred until it became a paste. The pH value was adjusted to 7 with a sodium hydroxide solution with a mass concentration of 1%, and the water bath was heated to 50°C. 30% hydrogen peroxide was slowly added to the system by a syringe pump (the amount of hydrogen peroxide added was 20% of the mass of starch). The pH value was kept constant during this process. After the addition was completed, the solution in the system reacted for 4 hours, and the obtained solution was filtered, washed with distilled water and dried to finally obtain hydrogen peroxide oxidized starch (OS) solid.

[0030] Example 1

[0031] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 80°C. The starch was stirred and gelatinized for 0.5h. Then, a 0.5% ammonium cerium nitrate solution was added with a syringe pump, and the mass of ammonium cerium nitrate was 3% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% MA solution was slowly injected into the system with a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 4:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 6h. After the reaction was completed, the product was dried in a 90°C oven for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0032] Example 2

[0033] The hydrogen peroxide oxidized starch obtained in Preparation Example 2 was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 80°C. The starch was stirred and gelatinized for 0.5h. Then, a 0.5% cerium ammonium nitrate solution was added with a syringe pump, and the mass of cerium ammonium nitrate was 3% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% MA solution was slowly injected into the system using a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 4:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 6h. After the reaction was completed, the product was dried in a 90°C oven for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0034] Example 3

[0035] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 80°C. The starch was stirred and gelatinized for 0.5h. Then, a 0.5% cerium ammonium nitrate solution was added with a syringe pump, and the mass of cerium ammonium nitrate was 3% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 15% mass percentage MA solution was slowly injected into the system using a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 5:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 6h. After the reaction was completed, the product was dried in a 90°C oven for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0036] Example 4

[0037] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 75°C. The starch was stirred and gelatinized for 0.5h. Then, a 0.5% cerium ammonium nitrate solution was added with a syringe pump, and the mass of cerium ammonium nitrate was 3% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% MA solution was slowly injected into the system with a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 4:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 6h. After the reaction was completed, the product was dried in a 90°C oven for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0038] Example 5

[0039] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 15 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 80°C. The starch was stirred and gelatinized for 0.5h. Then, a 0.5% cerium ammonium nitrate solution was added with a syringe pump, and the mass of cerium ammonium nitrate was 4% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% mass percentage MA solution was slowly injected into the system using a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 4:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 6h. After the reaction was completed, the product was dried in a 90°C oven for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0040] Example 6

[0041] The hydrogen peroxide oxidized starch obtained in Preparation Example 1 was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 80°C. The starch was stirred and gelatinized for 0.5h. Then, a 0.5% cerium ammonium nitrate solution was added with a syringe pump, and the mass of cerium ammonium nitrate was 3% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% MA solution was slowly injected into the system with a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 2:1, and the dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 6h. After the reaction was completed, the product was dried in a 90°C oven for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0042] Comparative Example 1

[0043] The hydrogen peroxide oxidized starch was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask. In a suspension state, the temperature was raised to 60°C, and the starch was stirred and gelatinized for 0.5h. Then, a 0.5% cerium ammonium nitrate solution was added with a syringe pump. The mass of cerium ammonium nitrate was 3% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% MA solution was slowly injected into the system with a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 4:1. The dripping time was 0.5h. After the dripping was completed, the reaction was continued for 6h. After the reaction was completed, the product was dried in an oven at 90°C for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0044] Comparative Example 2

[0045] The hydrogen peroxide oxidized starch was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 40°C. The starch was stirred and gelatinized for 0.5h. Then, a 0.5% cerium ammonium nitrate solution was added with a syringe pump. The mass of cerium ammonium nitrate was 3% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% mass percentage MA solution was slowly injected into the system with a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 4:1. The dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 6h. After the reaction was completed, the product was dried in an oven at 90°C for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0046] Comparative Example 3

[0047] The hydrogen peroxide oxidized starch was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 80°C. The starch was stirred and gelatinized for 0.5h. Then, a 0.5% cerium ammonium nitrate solution was added with a syringe pump. The mass of cerium ammonium nitrate was 3% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% mass percentage MA solution was slowly injected into the system with a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 4:1. The dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 90°C for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0048] Comparative Example 4

[0049] Hydrogen peroxide oxidized starch was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 80°C. The starch was stirred and gelatinized for 0.5h. Then, a 0.5% cerium ammonium nitrate solution was added with a syringe pump. The mass of cerium ammonium nitrate was 3% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% MA solution was slowly injected into the system with a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 2:1. The addition time was 0.5h. After the addition was completed, the reaction was continued for 3h. After the reaction was completed, the product was dried in an oven at 90°C for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0050] Comparative Example 5

[0051] The hydrogen peroxide oxidized starch was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 80°C. The starch was stirred and gelatinized for 0.5h. Then, a 0.5% cerium ammonium nitrate solution was added with a syringe pump. The mass of cerium ammonium nitrate was 8% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% mass percentage MA solution was slowly injected into the system with a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 1:1. The dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 6h. After the reaction was completed, the product was dried in an oven at 90°C for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0052] Comparative Example 6

[0053] The hydrogen peroxide oxidized starch was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 80°C. The starch was stirred and gelatinized for 0.5h. Then, a 0.5% cerium ammonium nitrate solution was added with a syringe pump. The mass of cerium ammonium nitrate was 10% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% mass percentage MA solution was slowly injected into the system again using a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 7:1. The dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 6h. After the reaction was completed, the product was dried in an oven at 90°C for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0054] Comparative Example 7

[0055] The hydrogen peroxide oxidized starch was added to distilled water equivalent to 10 times its mass, and magnetic stirring was performed in a four-necked flask to form a suspension state. Nitrogen was introduced into the system, and the temperature was raised to 80°C. The starch was stirred and gelatinized for 0.5h. Then, a 0.5% cerium ammonium nitrate solution was added with a syringe pump. The mass of cerium ammonium nitrate was 5% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% mass percentage MA solution was slowly injected into the system with a syringe pump. The mass ratio of maleic anhydride to oxidized starch was 1:1. The dropwise addition time was 0.5h. After the dropwise addition was completed, the reaction was continued for 4h. After the reaction was completed, the product was dried in an oven at 90°C for 24h to obtain a solid product. The solid product was washed with acetone and dried again to obtain the final product.

[0056] Comparative Example 8

[0057] The same as Example 1, except that the hydrogen peroxide oxidized starch is prepared by the following method:

[0058] A certain amount of soluble corn starch and 10 times of distilled water were added to a four-necked flask and stirred until it became a paste. The pH value was adjusted to 4 with a 1% sodium hydroxide solution, heated to 30°C in a water bath, and 30% hydrogen peroxide was slowly added to the system by a syringe pump (the amount of hydrogen peroxide added was 20% of the mass of starch). The pH value was kept constant during this process. After the addition was completed, the solution in the system reacted for 4 hours, and the obtained solution was filtered, washed with distilled water, and dried to finally obtain hydrogen peroxide oxidized starch OS solid.

[0059] Comparative Example 9

[0060] The same as Example 1, except that the hydrogen peroxide oxidized starch is prepared by the following method:

[0061] A certain amount of soluble corn starch and 10 times of distilled water were added to a four-necked flask and stirred until it became a paste. A sodium hydroxide solution with a mass concentration of 1% was used to adjust the pH value to about 9, and the water bath was heated to 50°C. A 30% hydrogen peroxide solution (the amount of hydrogen peroxide added was 20% of the mass of starch) was slowly added to the system by a syringe pump. The pH value was kept constant during this process. After the addition was completed, the solution in the system reacted for 4 hours, and the obtained solution was filtered, washed with distilled water, and dried to finally obtain hydrogen peroxide oxidized starch OS solid.

[0062] Comparative Example 10

[0063] The same as Example 1, except that the hydrogen peroxide oxidized starch is prepared by the following method:

[0064] A certain amount of soluble corn starch and distilled water were added to a four-necked flask and stirred until it became a paste. A 1% sodium hydroxide solution was used to adjust the pH value to about 6, and the water bath was heated to 30°C. A 30% hydrogen peroxide solution was slowly added to the system by a syringe pump (the amount of hydrogen peroxide added was 20% of the mass of the starch). The pH value was kept constant during this process. After the addition was completed, the solution in the system reacted for 4 hours, and the obtained solution was filtered, washed with distilled water, and dried to finally obtain hydrogen peroxide oxidized starch OS solid.

[0065] Comparative Example 11

[0066] Sodium hypochlorite is used as starch oxidant, the temperature is controlled at 40℃, and the pH is about 8. After 2 hours of reaction, crude sodium chlorate oxidized starch is obtained, which is added to distilled water equivalent to 10 times its mass, and magnetic stirring is carried out in a four-necked flask. It is in a suspension state, nitrogen is introduced into the system, and the temperature is raised to 80℃. The starch is stirred and gelatinized for 0.5 hours. Then, a 0.5% ammonium cerium nitrate solution is added with a syringe pump. The mass of ammonium cerium nitrate is 3% of the total mass of oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% MA solution is slowly injected into the system with a syringe pump. The mass ratio of maleic anhydride to oxidized starch is 4:1. The dropwise addition time is 0.5 hours. After the dropwise addition is completed, the reaction is carried out for 6 hours. After the reaction is completed, the product is dried in a 90℃ oven for 24 hours to obtain a solid product. The solid product is washed with acetone and dried again to obtain the final product.

[0067] Comparative Example 12

[0068] Hydrogen peroxide oxidized starch was prepared according to the method of Preparation Example 1, and the hydrogen peroxide oxidized starch was mechanically mixed with maleic anhydride at a mass ratio of 4:1, and the product was obtained after mixing evenly.

[0069] Test Example 1

[0070] The anti-scaling performance, dispersibility and sustained-release performance of the polymers obtained in the examples and comparative examples were evaluated respectively.

[0071] The performance of the agent in inhibiting calcium carbonate scale and calcium phosphate scale was evaluated according to GB / T16632-2008 "Determination of scale inhibition performance of water treatment agents - Calcium carbonate deposition method" and GB / T22626-2008 "Determination of scale inhibition performance of water treatment agents - Calcium phosphate deposition method" respectively; the dispersion performance was evaluated by measuring the dispersion performance of the agent on iron oxide (with the transmittance of distilled water as 100% as the standard, the smaller the transmittance, the better the dispersion performance); the corrosion inhibition effect reached the national standard GB50050-2017 Industrial Circulating Cooling Water Treatment Design Code, and the corrosion rate of carbon steel was <0.075mm / a.

[0072] (1) Determination of scale inhibition performance of calcium carbonate

[0073] The experiment uses prepared water and non-evaporative concentration to determine the CaCO3 resistance performance. 2+ and HCO3 - The concentrations were 600mg / L and 1200mg / L (calculated as CaCO3), respectively. A certain amount of water treatment agent was added to 500ml of water sample, and then placed in a constant temperature water bath at 80℃ and kept at constant temperature for 10 hours. Then cooled to room temperature, the upper clear layer was taken and the Ca content was determined by EDTA method. 2+ The scale inhibition rate is calculated as shown in formula (1).

[0074] (1)

[0075] Where: C0 is the Ca content in the solution after the heating experiment without adding scale inhibitor and dispersant 2+ Content, mg / L;

[0076] C1 is the Ca content in the solution after the heating experiment when adding scale inhibitor and dispersant 2+ Content, mg / L;

[0077] C2 is the Ca content of the experimental water without adding scale inhibitor and dispersant and without heating 2+ Content, mg / L.

[0078] (2) Determination of scale inhibition performance of calcium phosphate

[0079] The experiment uses prepared water and non-evaporative concentration to determine the Ca3(PO4)2 resistance. 2+ The concentration is 250mg / L (calculated as CaCO3), PO4 3- The concentration is 150mg / L. A certain amount of water treatment agent is added to 500ml of water sample. The pH value of the solution is 9 (adjusted with sodium tetraborate). It is placed in a constant temperature water bath at 80℃ and kept at constant temperature for 10 hours. Then it is cooled to room temperature, and the upper clear layer is taken and the PO4 in it is measured by a visible spectrophotometer. 3- The scale inhibition rate is calculated as shown in formula (2).

[0080] (2)

[0081] Where: C0 is the PO4 in the solution after the heating test without adding scale inhibitor dispersant 3- Content, mg / L;

[0082] C1 is the PO4 in the solution after the heating test when adding scale inhibitor and dispersant 3- Content, mg / L;

[0083] C2 is the PO4 of the experimental water without adding antiscaling dispersant and heating 3- Content, mg / L.

[0084] (3) Determination of the performance of dispersed Fe2O3

[0085] Using analytically pure anhydrous calcium chloride and ammonium ferrous sulfate as reagents, the following experimental water samples were prepared: Ca 2+ The concentration is 150 mg / L (calculated as CaCO3), Fe 2+The concentration is 10 mg / L. A certain amount of water treatment agent is added to 500 ml of water sample. The pH value of the solution is 9 (adjusted with sodium tetraborate). After strong stirring for 15 minutes, it is placed in a constant temperature water bath at 50°C for 5 hours. After cooling to room temperature, the upper layer of solution is taken and its transmittance T is measured at 450 nm with a visible spectrophotometer. The smaller the transmittance, the better the dispersion effect (taking distilled water as a reference, its transmittance is 100%).

[0086] (4) Determination of corrosion rate

[0087] The rotating coupon weight loss method was adopted, referring to the national standard GB / T 18175-2014, using a rotating coupon corrosion tester, A3 carbon steel sheet (50mm×25mm×2mm), test time: 72h; test temperature: 40℃; rotation speed: 75r / min, the calculation formula of the corrosion rate X1 expressed in mm / a is:

[0088]

[0089] Where: W is the weight of the test piece before the test, g; W0 is the weight of the test piece after the test, g; A is the surface area of ​​the test piece, 28cm 2 ; D is the density of the test piece, carbon steel is 7.850g / cm 3 ; T is the test time of the specimen, 72h.

[0090] The following table shows the national standard for the corrosion rate of carbon steel. After adding the agent, the corrosion rate of the solution on carbon steel should be less than 0.075mm / a.

[0091] National Standard for Corrosion Rate of Carbon Steel

[0092]

[0093] The test results of various properties of the polymers obtained in the examples and comparative examples are shown in Table 1.

[0094] Table 1 Performance test results

[0095]

[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A scale dispersing corrosion inhibitor, characterized in that It is obtained by copolymerizing maleic anhydride and hydrogen peroxide oxidized starch, the mass ratio of maleic anhydride to hydrogen peroxide oxidized starch is 4:1, and the polymerization method is as follows: The hydrogen peroxide oxidized starch is added to distilled water equivalent to 10 times its mass, and magnetic stirring is performed in a four-necked flask to form a suspension state. Nitrogen is introduced into the system, and the temperature is raised to 80° C. The starch is stirred and gelatinized for 0.5 h. Then, a 0.5% ammonium cerium nitrate solution is added by a syringe pump, and the mass of the ammonium cerium nitrate is 3% of the total mass of the oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% MA solution is slowly injected into the system by a syringe pump, and the dripping time is 0.5 h. After the dripping is completed, the reaction is carried out for 6 hours; After the reaction was completed, the product was dried in an oven at 90°C for 24 hours to obtain; The preparation method of the hydrogen peroxide oxidized starch is as follows: A certain amount of soluble corn starch and distilled water equivalent to 10 times its mass were added to a four-necked flask, stirred into a paste, and the pH value was adjusted to 6 with a sodium hydroxide solution with a mass concentration of 1%. The mixture was heated to 50°C in a water bath, and 30% hydrogen peroxide was slowly added to the system by a syringe pump. The amount of hydrogen peroxide added was 20% of the mass of the starch. The pH value was kept constant during the process. After the addition was completed, the solution in the system reacted for 4 hours, and the obtained solution was filtered, washed with distilled water and dried to finally obtain hydrogen peroxide oxidized starch solid.

2. A method for preparing the scale-dispersing corrosion inhibitor according to claim 1, characterized in that: It includes the following steps: A certain amount of soluble corn starch and distilled water equivalent to 10 times the mass of the soluble corn starch were added to a four-necked flask, and the mixture was stirred to form a paste. A sodium hydroxide solution with a mass concentration of 1% was used to adjust the pH value to 6. The mixture was heated to 50° C. in a water bath. 30% hydrogen peroxide was slowly added dropwise to the system by a syringe pump. The amount of hydrogen peroxide added was 20% of the mass of the starch. The pH value was kept constant during the process. After the addition was completed, the solution in the system was reacted for 4 hours. The obtained solution was filtered, washed with distilled water, and dried to finally obtain hydrogen peroxide oxidized starch solid. The hydrogen peroxide oxidized starch is added to distilled water with a mass equivalent to 10 times of the hydrogen peroxide, and magnetic stirring is performed in a four-necked flask to form a suspension state. Nitrogen is introduced into the system, and the temperature is raised to 80° C. The starch is stirred and gelatinized for 0.5 h. Then, a 0.5% ammonium cerium nitrate solution is added by a syringe pump, and the mass of the ammonium cerium nitrate is 3% of the total mass of the oxidized starch and maleic anhydride. After 15 minutes of initiation, a 10% MA solution is slowly injected into the system by a syringe pump, the mass ratio of maleic anhydride to oxidized starch is 4:1, the dropping time is 0.5 h, and the reaction is carried out for 6 hours after the dropping is completed; after the reaction is completed, the product is dried in an oven at 90° C. for 24 hours to obtain.

3. Use of the scale inhibitor, dispersant and slow-release agent as claimed in claim 1 as a water treatment agent in industrial circulating cooling water.

Citation Information

Patent Citations

  • Preparation method of non-phosphorus composite scale inhibitor

    CN102452723A

  • Novel phosphorus-free corrosion and scale inhibitor and preparation method thereof

    CN110342654A

  • Method for synthesizing phosphorus-free corrosion-inhibition scale inhibitor for water treatment from natural products

    CN101768244A

  • Scale inhibitor for boiler and water supply pipeline

    CN104692545A

  • Phosphorus-free scale inhibitor, and preparation method and application thereof

    CN111362429A