A flame-retardant PP that is not easy to ignite and its preparation method

Through the special structure of coconut shell loaded hydrotalcite and glass fiber, combined with gas phase and solid phase flame retardants, the problems of polypropylene flammability and insufficient mechanical properties are solved, and the efficient flame retardant and mechanical properties are achieved, which significantly improves resistance Flame retardant effect of burning PP.

CN118126454BActive Publication Date: 2024-11-26ZHONGSHAN QIRUIDA ENG PLASTICS IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410352710.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-26
Publication Date
2024-11-26
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

Polypropylene materials are flammable and combustion produce harmful smoke and gases, limiting their application in areas with high flame retardant performance requirements. The existing filler addition is large and weakens the mechanical properties of the substrate.

Method used

Coconut shells are used as carrier to load hydrotalcite, combined with glass fibers, to form a special structure to improve compatibility and mechanical properties, and reduce harmful effects through the synergistic effects of decabromodiphenylethane, antimony trioxide, ammonium polyphosphate and melamine. Gas generation, combining gas phase and solid phase flame retardant mode.

Benefits of technology

It achieves the excellent flame retardant performance and mechanical properties of polypropylene materials, reduces the amount of hydrotalcite, effectively dilutes the flame and absorbs harmful gases, enhances the mechanical interlocking effect, and improves the flame retardant effect of flame retardant PP.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present application relates to the field of polypropylene materials, and more specifically, it relates to a flame-retardant PP that is not easy to ignite and a preparation method thereof. A flame-retardant PP that is not easy to ignite, according to mass parts, includes the following raw materials: 90-110 parts of polypropylene, 1-5 parts of decabromodiphenylethane, 1-5 parts of antimony trioxide, 1-5 parts of ammonium polyphosphate, 1-5 parts of melamine, 0.01-1 parts of antioxidant, 1-10 parts of filler, 1-10 parts of glass fiber, 1-3 parts of coconut shell, 0.5-1.5 parts of hydrotalcite, and 1-3 parts of coupling agent. The flame-retardant PP prepared in the present application has the advantages of good mechanical properties, excellent flame retardant effect, not easy to ignite, and low smoke after ignition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of polypropylene materials, and more specifically, to a flame-retardant PP that is not easy to ignite and a preparation method thereof. Background Art

[0002] Polypropylene (PP) is a polymer material with a low limiting oxygen index (LOI) and is easy to burn. During the combustion process, PP will quickly generate a large amount of heat and gas, causing the fire to spread rapidly, increasing the risk of fire. In addition, when PP burns, it will produce a large amount of smoke and toxic gases, such as hydrogen chloride, which are harmful to human health and the environment. Especially in a closed or poorly ventilated environment, these harmful gases are more dangerous. Due to the flammability of PP and the harmfulness of its combustion products, its application in some fields with high requirements for flame retardancy is limited, such as automobiles, construction, electronics and electrical fields.

[0003] In the prior art, fillers such as hydrotalcite may be added to polypropylene to improve its flame retardant effect. However, the flame retardant effect of such fillers themselves is not obvious. If the ideal flame retardant effect is to be achieved, a very high addition amount (more than 40wt%) is usually required, which will significantly weaken the mechanical properties of the PP matrix. Therefore, there is still room for improvement. Summary of the invention

[0004] In order to improve the flame retardant effect of polypropylene, the present application provides a flame retardant PP that is not easy to ignite and a preparation method thereof.

[0005] In the first aspect, the present application provides a flame-retardant PP that is not easy to ignite, using the following technical solution:

[0006] A flame-retardant PP which is not easy to ignite comprises the following raw materials in parts by mass: 90-110 parts of polypropylene, 1-5 parts of decabromodiphenylethane, 1-5 parts of antimony trioxide, 1-5 parts of ammonium polyphosphate, 1-5 parts of melamine, 0.01-1 parts of antioxidant, 1-10 parts of filler, 1-10 parts of glass fiber, 1-3 parts of coconut shell, 0.5-1.5 parts of hydrotalcite and 1-3 parts of coupling agent.

[0007] By adopting the above technical scheme, coconut shell is used as a carrier to load hydrotalcite, forming a special structure, so that hydrotalcite is not easy to agglomerate, which is conducive to improving the compatibility and coordination of hydrotalcite and polypropylene matrix, and can also give full play to the effect of hydrotalcite. At the same time, the special structure is combined with the network structure of glass fiber, spreads and distributes in the polypropylene system, is evenly dispersed, and is not easy to fall off. Since hydrotalcite plays a synergistic role in the polypropylene system in the form of a special structure, the amount of hydrotalcite can be greatly reduced, so that polypropylene has excellent mechanical properties, and at the same time, it can also be well flame retardant and not easy to ignite.

[0008] When a fire occurs, hydrotalcite decomposes under heat, releasing a large amount of water and carbon dioxide, which effectively dilutes the concentration of combustible gases in the flame and stops the combustion. The carbonate ions in hydrotalcite can also effectively absorb gases such as hydrogen chloride produced by the combustion of PP, further alleviating the combustion situation.

[0009] At the same time, coconut shell and hydrotalcite can effectively synergistically promote the formation of a porous carbon layer, expand and flame retardant, and coat the surface of the substrate to isolate heat and oxygen.

[0010] Flame retardant PP has excellent flame retardant properties through a variety of methods.

[0011] Decabromodiphenylethane, antimony trioxide, ammonium polyphosphate, and melamine combine gas phase flame retardancy with solid phase flame retardancy, which can reduce the amount of harmful gases produced during combustion and further help improve the flame retardant effect of flame retardant PP.

[0012] In addition, the combination of coconut shell with hydrotalcite and glass fiber can enhance the molecular force between coconut shell and polypropylene molecules, improve the mechanical interlocking effect, and promote the polypropylene molecular chains to be arranged in a more regular manner to improve the mechanical properties.

[0013] Preferably, when the hydrotalcite is a modified hydrotalcite, it comprises the following modified raw materials: ordinary hydrotalcite, dodecasodium phytate, and tartaric acid, and the molar ratio of ordinary hydrotalcite, dodecasodium phytate, and tartaric acid is 1:(0.3-0.6):(0.1-0.3).

[0014] By adopting the above technical scheme, ordinary hydrotalcite is modified with dodecasodium phytate and tartaric acid. Dodecasodium phytate and tartaric acid are quickly and strongly attracted between the electropositive hydrotalcite layers, and stably intercalate and assemble into the hydrotalcite layers, so that the modified hydrotalcite has higher hydrophobicity.

[0015] The interlayer spacing of the modified hydrotalcite becomes larger and the reaction active sites become more. When encountering a fire situation, it can respond faster and more forcefully, thereby improving the flame retardant effect of flame retardant PP.

[0016] In addition, the structure of the modified hydrotalcite has changed, so it can be loaded onto the coconut shell more and more firmly, and is not easy to fall off, which effectively increases the reaction area.

[0017] Preferably, the preparation method of the modified hydrotalcite comprises the following steps:

[0018] Step a: ordinary hydrotalcite is mixed with water to prepare liquid a; dodecasodium phytate, tartaric acid and water are mixed to prepare liquid b;

[0019] Step b: Mix solution a and solution b, maintain the pH at 6-7; and stir at 55-65°C for 1-2h;

[0020] Step c: solid-liquid separation, the solid part is the modified hydrotalcite.

[0021] Preferably, the mass fraction of the coconut shell is 2-3 parts, and the mass fraction of the modified hydrotalcite is 0.5-1 part.

[0022] By adopting the above technical solution, the dosage relationship between coconut shell and modified hydrotalcite is further limited. Under this relationship, the modified hydrotalcite can be stably loaded on the coconut shell without causing waste; it also helps to improve the mechanical properties of flame-retardant PP.

[0023] Preferably, the filler is a mixture of one or more of talc, mica, calcium carbonate and barium sulfate.

[0024] In a second aspect, the present application provides a method for preparing a flame-retardant PP that is not easy to ignite, using the following technical solution:

[0025] A method for preparing a flame-retardant PP that is not easy to ignite, comprising the following steps:

[0026] Step 1: calcining the coconut shell at a temperature of 450-550° C. to obtain calcined coconut shell;

[0027] Step 2: Mix the calcined coconut shell with water to prepare a suspension;

[0028] Step 3: Add hydrotalcite to the suspension and mix until uniform;

[0029] Step 4: placing the material of step 3 at 150-180°C for aging for 45-70 minutes;

[0030] Step 5: Separate the solid and liquid of the material in step 4 and take the solid part; the solid part is a composite material;

[0031] Step 6: The composite material, polypropylene, decabromodiphenylethane, antimony trioxide, ammonium polyphosphate, melamine, antioxidant, filler, glass fiber and coupling agent are mixed until uniform, and then blended at 190-210° C., extruded and granulated to obtain flame-retardant PP.

[0032] By adopting the above technical solution, coconut shell is prepared into biochar to load hydrotalcite to form a specific structure, and cooperate with glass fiber to have good compatibility with the polypropylene matrix. During combustion, the presence of coconut shell also increases the flow resistance of polypropylene after heating, consuming heat energy; the hydroxyl group of hydrotalcite loaded on coconut shell acts as a carbonizing agent to further block heat; the remaining heat is quickly dispersed through the network structure of glass fiber; and flame-retardant PP is not easy to ignite through various means.

[0033] Preferably, in step 1, the calcination time is 15-30 min.

[0034] By adopting the above technical solution, the calcination time of step 1 is limited, so that the coconut shell will not be excessively carbonized or not carbonized, and the target carrier is formed to better carry the hydrotalcite.

[0035] Preferably, in step 6, the blending time is 5-15 min.

[0036] By adopting the above technical solution, the blending time is further limited at a specific temperature, so that various raw materials can be mixed more fully to improve the mechanical properties and flame retardant effects.

[0037] In summary, this application has the following beneficial effects:

[0038] 1. Since the present application adopts coconut shell, hydrotalcite, glass fiber and other raw materials to form a specific structure, the amount of hydrotalcite can be effectively reduced, so that the flame-retardant PP has higher mechanical properties; at the same time, it also has excellent flame-retardant effect.

[0039] 2. In this application, decabromodiphenylethane, antimony trioxide, ammonium polyphosphate and melamine are preferably used to organically combine gas phase flame retardancy and solid phase flame retardancy, which can effectively reduce the amount of harmful gases produced during combustion and assist in improving the flame retardant effect of flame retardant PP. DETAILED DESCRIPTION

[0040] The present application is further described in detail below with reference to the embodiments.

[0041] The raw materials used in the following examples and comparative examples are all commercially available products.

[0042] Example

[0043] Example 1

[0044] A flame-retardant PP which is not easy to ignite comprises the following raw materials: polypropylene, decabromodiphenylethane, antimony trioxide, ammonium polyphosphate, melamine, antioxidant, filler, glass fiber, coconut shell, hydrotalcite and coupling agent.

[0045] Polypropylene is commercially available. In this embodiment, it was purchased from Ningbo Lanchen Plastic Chemical Co., Ltd. with a model of T30S and a brand of Fude.

[0046] Hydrotalcite is commercially available, and in this embodiment, it was purchased from Nantong Runfeng Petrochemical Co., Ltd.

[0047] The antioxidant is antioxidant 1010.

[0048] The filler is talc.

[0049] The coupling agent is KH-560.

[0050] The specific dosage is shown in Table 1.

[0051] The present application also provides a method for preparing a flame-retardant PP that is not easy to ignite, comprising the following steps:

[0052] Step 1: Clean and dry the coconut shells, and crush them into 100 mesh.

[0053] Then the crushed coconut shell was placed in a reactor and calcined at 500°C for 20 minutes.

[0054] After being taken out, the coconut shell was cooled to room temperature, washed repeatedly with deionized water until neutral, and dried in a drying oven at 60° C. to obtain calcined coconut shell.

[0055] Step 2: Mix the calcined coconut shell with water to prepare a suspension. The mixing ratio of the calcined coconut shell to water is 1:15.

[0056] Step 3: Add hydrotalcite to the suspension and mix at a high speed of 800 r / min until uniform. Then keep stirring for 1 hour.

[0057] Step 4: Place the material from step 3 in a reactor and age it at 160°C for 60 minutes.

[0058] Step 5: Separate the solid and liquid of the material in step 4, take the solid part, repeatedly rinse the solid part with deionized water until it is neutral, and then dry it in hot air at 60°C to constant weight. The solid part is a composite material.

[0059] Step 6: The composite material, polypropylene, decabromodiphenylethane, antimony trioxide, ammonium polyphosphate, melamine, antioxidant, filler, glass fiber and coupling agent are mixed until uniform. Then, the mixture is placed in a twin-screw extruder and blended at 200° C. for 10 minutes. After extrusion and granulation, flame-retardant PP is obtained.

[0060] Example 2

[0061] A flame-retardant PP that is not easy to ignite, which is different from Example 1 in that the amounts of various raw materials used are different.

[0062] A method for preparing a flame-retardant PP that is not easy to ignite, which is different from Example 1 in that:

[0063] In step 1, the calcination temperature is 450° C. and the calcination time is 30 min.

[0064] In step 3, the aging treatment temperature is 150° C. and the treatment time is 70 min.

[0065] In step 6, the blending temperature is 190° C. and the blending time is 15 min.

[0066] The specific dosage is shown in Table 1.

[0067] Example 3

[0068] A flame-retardant PP that is not easy to ignite, which is different from Example 1 in that the amounts of various raw materials used are different.

[0069] A method for preparing a flame-retardant PP that is not easy to ignite, which is different from Example 1 in that:

[0070] In step 1, the calcination temperature is 550° C. and the calcination time is 15 min.

[0071] In step 3, the aging treatment temperature is 18° C. and the treatment time is 45 min.

[0072] In step 6, the blending temperature is 210° C. and the blending time is 5 min.

[0073] The specific dosage is shown in Table 1.

[0074] Table 1

[0075] Category Example 1 Example 2 Example 3 Polypropylene (kg) 100 90 110 Decabromodiphenylethane(kg) 3 1 5 Antimony trioxide (kg) 2 5 1 Ammonium polyphosphate (kg) 3 1 5 Melamine(kg) 2 5 1 Antioxidant(kg) 0.6 0.01 1 Filling(kg) 6 1 10 Glass fiber(kg) 3.5 10 1 Coconut shell (kg) 2.5 3 1 Hydrotalcite(kg) 0.8 1.5 0.5 Coupling agent(kg) 1.5 3 1

[0076] Example 4

[0077] A flame-retardant PP that is not easy to ignite. The difference from Example 1 is that the hydrotalcite is modified hydrotalcite, and the amount of the modified hydrotalcite is 0.8 kg.

[0078] The modified raw materials of the modified hydrotalcite include: common hydrotalcite, dodecasodium phytate and tartaric acid, and the molar ratio of the common hydrotalcite, dodecasodium phytate and tartaric acid is 1:0.5:0.2.

[0079] The preparation method of modified hydrotalcite comprises the following steps:

[0080] Step a: ordinary hydrotalcite is mixed with water to prepare liquid a; dodecasodium phytate, tartaric acid and water are mixed to prepare liquid b.

[0081] The mass ratio of ordinary hydrotalcite to water is 1:10. The mass ratio of the total amount of dodecasodium phytate and tartaric acid to water is 1:20.

[0082] Step b: Mix solution a and solution b, and use a pH adjuster to maintain the pH at 6.5.

[0083] Then the mixture was stirred at 60°C for 1.5 h.

[0084] Step c: solid-liquid separation, the solid part is washed with deionized water to neutrality, and dried in hot air at 40° C. to constant weight, and the solid part is the modified hydrotalcite.

[0085] Example 5

[0086] A flame retardant PP that is not easy to ignite, which is different from Example 4 in that:

[0087] The amount of coconut shell is 2 kg and the amount of modified hydrotalcite is 0.5 kg.

[0088] In the modified raw materials of the modified hydrotalcite, the molar ratio of common hydrotalcite, dodecasodium phytate and tartaric acid is 1:0.3:0.1.

[0089] In step b, the pH was maintained at 6 and the mixture was stirred at 55° C. for 2 h.

[0090] Example 6

[0091] A flame retardant PP which is not easy to ignite, which is different from Example 4 in that:

[0092] The amount of coconut shell is 3 kg and the amount of modified hydrotalcite is 1 kg.

[0093] In the modified raw materials of the modified hydrotalcite, the molar ratio of common hydrotalcite, dodecasodium phytate and tartaric acid is 1:0.6:0.3.

[0094] In step b, the pH was maintained at 7 and the mixture was stirred at 65° C. for 1 h.

[0095] Example 7

[0096] A flame-retardant PP that is not easy to ignite, which is different from Example 4 in that the molar ratio of ordinary hydrotalcite, dodecasodium phytate and tartaric acid is 1:1:1.

[0097] Example 8

[0098] A flame retardant PP that is not easy to ignite, which is different from Example 4 in that:

[0099] The modified raw materials of the modified hydrotalcite include: ordinary hydrotalcite and sodium dodecyl sulfate, and the molar ratio of the ordinary hydrotalcite to the sodium dodecyl sulfate is 1:0.7.

[0100] The preparation method of modified hydrotalcite comprises the following steps:

[0101] Step a: ordinary hydrotalcite is mixed with water to prepare liquid a; sodium dodecyl sulfate is mixed with water to prepare liquid b.

[0102] The mass ratio of ordinary hydrotalcite to water is 1:10. The mass ratio of sodium lauryl sulfate to water is 1:20.

[0103] Step b: Mix solution a and solution b, and use a pH adjuster to maintain the pH at 6.5.

[0104] Then the mixture was stirred at 60°C for 1.5 h.

[0105] Step c: solid-liquid separation, the solid part is washed with deionized water to neutrality, and dried in hot air at 40° C. to constant weight, and the solid part is the modified hydrotalcite.

[0106] Comparative Example

[0107] Comparative Example 1

[0108] A flame-retardant PP that is not easy to ignite, which is different from Example 1 in that hydrotalcite is replaced by brucite.

[0109] Comparative Example 2

[0110] A flame-retardant PP that is not easy to ignite, which is different from Example 1 in that coconut shell is replaced by wheat straw.

[0111] Comparative Example 3

[0112] A flame-retardant PP that is not easy to ignite, which is different from Example 1 in that the hydrotalcite is 0.8 kg, the coconut shell is 3.5 kg, and the glass fiber is 2.5 kg.

[0113] Comparative Example 4

[0114] A method for preparing flame-retardant PP that is not easy to ignite, which is different from Example 1 in that the calcination temperature in step 1 is 700°C.

[0115] Comparative Example 5

[0116] A flame-retardant PP that is not easy to ignite, which is different from Example 4 in that the coconut shell is 3.2 kg and the modified hydrotalcite is 0.1 kg.

[0117] Comparative Example 6

[0118] A flame-retardant PP that is not easy to ignite, which is different from Example 4 in that the coconut shell is 0.1 kg and the modified hydrotalcite is 3.2 kg.

[0119] Comparative Example 7

[0120] A flame-retardant PP that is not easy to ignite, which is different from Example 4 in that hydrotalcite is replaced by brucite.

[0121] Comparative Example 8

[0122] A flame-retardant PP that is not easy to ignite, which is different from Example 4 in that coconut shell is replaced by wheat straw.

[0123] Performance testing

[0124] 1. Mechanical properties: The tensile strength of the flame-retardant PP of Examples 1-8 and Comparative Examples 1-8 was tested with reference to GB / T 1040-2006. The tensile rate was 20 mm / min. The tensile strength was recorded in Table 2.

[0125] 2. Combustion performance:

[0126] 1) 850°C glow-wire flammability index test: The flame-retardant PP of Examples 1-8 and Comparative Examples 1-8 were tested with reference to GB / T 5169.12-2006 “Fire hazard tests for electric and electronic products Part 12: Glow-wire / hot-wire basic test methods - Glow-wire flammability test methods for materials”, and the results were recorded in Table 2.

[0127] 2) Smoke generation detection: The flame retardant PP of Examples 1-8 and Comparative Examples 1-8 were tested using a cone calorimeter, and the total amount of smoke generated was recorded in Table 2. The specific testing standard refers to ASTM E-1354.

[0128] Thermal radiation power is 50kW / m 2 , the sample size is 100*100*30mm.

[0129] 3) Limiting oxygen index test: The flame retardant PP of Examples 1-8 and Comparative Examples 1-8 were tested with reference to GB / T 2406.2-2009 "Determination of combustion behavior of plastics by oxygen index method Part 2: Room temperature test", and the sample strip size was 100 mm*6.5 mm*3.2 mm.

[0130] Table 2

[0131]

[0132] According to the comparison of the test data of Examples 1-3 and Comparative Examples 1-3 in Table 2, it can be seen that with the combination of glass fiber, coconut shell and hydrotalcite, the flame retardant PP has a high tensile strength and is difficult to ignite. Even if it is ignited, the smoke emission is low. If the raw materials are replaced with other raw materials or the special dosage combination between the three is destroyed, the performance of the flame retardant PP is greatly reduced, and it is impossible to have both good mechanical properties and flame retardant effects.

[0133] Comparative Example 4 is based on Example 1, but the calcination temperature of coconut shell is changed. According to the comparison of the test data of Example 1 and Comparative Example 4 in Table 2, it can be seen that the mechanical properties and flame retardant effect of the flame retardant PP of Comparative Example 4 are far inferior to those of Example 1. This is because after the calcination temperature is changed in Comparative Example 4, the carbonization degree of coconut shell is changed, and a specific carrier that is well matched with hydrotalcite cannot be formed, thereby affecting the performance of the flame retardant PP.

[0134] In Example 4-6, the hydrotalcite is modified on the basis of Example 1, and the interlayer spacing of the modified hydrotalcite is enlarged, and the coconut shell can be loaded more quickly and more, making the structure of glass fiber-coconut shell-modified hydrotalcite more stable and play a role in polypropylene. According to the comparison of the test data of Examples 1-3 and Examples 4-6 in Table 2, it can be seen that the flame-retardant PP of Examples 4-6 is superior in all aspects.

[0135] In Example 7-8, based on Example 4, the modified raw material type or dosage of the modified hydrotalcite is changed, so that the structure of the modified hydrotalcite changes, and its performance is reduced when applied to flame-retardant PP. This shows that specific raw materials can make the modified hydrotalcite better matched with coconut shells and the like, and play a role in polypropylene.

[0136] Comparative Examples 5-6 are based on Example 4, destroying the special dosage coordination effect between coconut shell and modified hydrotalcite; Comparative Examples 7-8 are based on Example 4, changing the selection of raw materials. According to the data in Table 2, these changes in conditions make it impossible for the modification method to achieve the ideal effect, and the flame retardant performance of PP is poor.

[0137] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A flame-retardant PP that is not easy to ignite, characterized in that: The raw materials include, by weight: 90-110 parts of polypropylene, 1-5 parts of decabromodiphenylethane, 1-5 parts of antimony trioxide, 1-5 parts of ammonium polyphosphate, 1-5 parts of melamine, 0.01-1 parts of antioxidant, 1-10 parts of filler, 1-10 parts of glass fiber, 1-3 parts of coconut shell, 0.5-1.5 parts of modified hydrotalcite, and 1-3 parts of coupling agent; The modified hydrotalcite comprises the following modified raw materials: ordinary hydrotalcite, dodecasodium phytate, and tartaric acid, wherein the molar ratio of ordinary hydrotalcite, dodecasodium phytate, and tartaric acid is 1: (0.3-0.6): (0.1-0.3); The preparation method of the modified hydrotalcite comprises the following steps: Step a: ordinary hydrotalcite is mixed with water to prepare liquid a; dodecasodium phytate, tartaric acid and water are mixed to prepare liquid b; Step b: Mix solution a and solution b, maintain the pH at 6-7; and stir at 55-65°C for 1-2h; Step c: solid-liquid separation, the solid part is the modified hydrotalcite; The method for preparing the flame-retardant PP which is not easy to ignite comprises the following steps: Step 1: calcining the coconut shell at a temperature of 450-550° C. to obtain calcined coconut shell; Step 2: Mix the calcined coconut shell with water to prepare a suspension; Step 3: Add the modified hydrotalcite into the suspension and mix until it is uniform; Step 4: placing the material of step 3 at 150-180°C for aging for 45-70 minutes; Step 5: Separate the solid and liquid of the material in step 4 and take the solid part; the solid part is a composite material; Step 6: The composite material, polypropylene, decabromodiphenylethane, antimony trioxide, ammonium polyphosphate, melamine, antioxidant, filler, glass fiber and coupling agent are mixed until uniform, and then blended at 190-210° C., extruded and granulated to obtain flame-retardant PP.

2. The flame-retardant PP that is not easy to ignite according to claim 1, characterized in that: The mass fraction of the coconut shell is 2-3 parts, and the mass fraction of the modified hydrotalcite is 0.5-1 part.

3. The flame-retardant PP that is not easy to ignite according to claim 1, characterized in that: The filler is a mixture of one or more of talc, mica, calcium carbonate and barium sulfate.

4. A method for preparing the flame-retardant PP that is not easy to ignite according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1: calcining the coconut shell at a temperature of 450-550° C. to obtain calcined coconut shell; Step 2: Mix the calcined coconut shell with water to prepare a suspension; Step 3: Add the modified hydrotalcite into the suspension and mix until it is uniform; Step 4: placing the material of step 3 at 150-180°C for aging for 45-70 minutes; Step 5: Separate the solid and liquid of the material in step 4 and take the solid part; the solid part is a composite material; Step 6: The composite material, polypropylene, decabromodiphenylethane, antimony trioxide, ammonium polyphosphate, melamine, antioxidant, filler, glass fiber and coupling agent are mixed until uniform, and then blended at 190-210° C., extruded and granulated to obtain flame-retardant PP.

5. The method for preparing the flame-retardant PP which is not easy to ignite according to claim 4, characterized in that: In the step 1, the calcination time is 15-30 minutes.