Preparation method of modified spherical alumina / wrinkled graphene / polysiloxane composite thermal conductive interface material
By combining modified spherical alumina and wrinkled graphene with polysiloxane, a continuous thermal conductivity pathway is formed, which solves the problem of uneven dispersion of thermally conductive fillers in the polymer matrix and achieves a high efficiency improvement in thermal conductivity, making it suitable for high-power electronic devices.
Patent Information
- Application Number
- CN202410302925.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-15
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-03-15
AI Technical Summary
Existing technologies struggle to achieve uniform dispersion of thermally conductive fillers and improve thermal conductivity within polymer matrices. Traditional metallic materials also suffer from insufficient insulation and mechanical properties, failing to meet the demands of modern thermal management.
Modified spherical alumina and wrinkled graphene are composited with polysiloxane. By preparing graphene powder loaded with nano-alumina and modified spherical alumina, and combining the mixing and thermosetting of graphene/spherical alumina/silicone prepolymer, a continuous thermally conductive pathway is formed, which improves the dispersibility and thermal conductivity of the filler in the polymer matrix.
The prepared modified spherical alumina/wrinkled graphene/polysiloxane composite material exhibits excellent thermal conductivity in both vertical and horizontal directions, with an in-plane thermal conductivity of 13.2 W/mK and an out-of-plane thermal conductivity of 3.063 W/mK. Moreover, the preparation method is simple and controllable, making it suitable for high-power electronic devices.
Smart Images

Figure CN118126525B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal conductive interface materials, and in particular relates to a preparation method of a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material. Background Art
[0002] With the development of the times, high-power electronic devices are becoming increasingly functional and their performance is improving. At the same time, heat dissipation has become a key issue restricting the miniaturization and high integration of electronic products. Modern electronics urgently needs efficient heat dissipation and thermal interface materials. In recent years, traditional thermal conductive materials such as metals have been unable to meet the requirements of modern thermal management due to problems such as weak insulation and poor mechanical properties. How to use simple methods to introduce high thermal conductivity fillers such as graphene, boron nitride, aluminum oxide, etc. into composite materials, and customize thermal conductive composite materials with certain microstructures and orientations according to actual needs, while making the composite materials have excellent mechanical properties is a major challenge and the future development direction of advanced thermal management materials. Physical blending is the most commonly used simple method for preparing high thermal conductivity polymer composite materials. However, in this method, achieving uniform dispersion of fillers is still a big challenge.
[0003] Therefore, it is necessary to develop a preparation method for modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material to solve the problems of complex preparation method, uneven dispersion of various thermal conductive fillers in the polymer matrix and poor thermal conductivity. Summary of the invention
[0004] The invention aims to provide a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material.
[0005] The technical solution of the present invention is:
[0006] A method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material, the method comprising:
[0007] (1) Preparation of graphene powder loaded with nano-alumina: Weighing graphene powder, adding nano-alumina ethanol dispersion, acetone, deionized water and polyvinyl pyrrolidone, stirring thoroughly, ultrasonically treating to obtain a uniform mixed solution, freezing and freeze-drying to obtain graphene powder loaded with nano-alumina;
[0008] (2) Preparation of modified spherical alumina powder: Spherical alumina of mixed particle sizes are mixed, deionized water and ethanol are added, and then a silane coupling agent is added to treat the surface of the spherical alumina, the pH is adjusted to be weakly acidic by glacial acetic acid, and the mixture is fully stirred, ultrasonically treated, and vacuum filtered at a constant temperature, washed with deionized water, and then dried to obtain modified spherical alumina powder;
[0009] (3) Preparation of graphene / spherical alumina / silica gel prepolymer: the graphene powder loaded with nano-alumina is uniformly mixed with the modified spherical alumina powder to obtain a graphene and spherical alumina mixed powder, vinyl-terminated polydimethylsiloxane, methyl hydrogen silicone oil, a catalyst, and an inhibitor are weighed to obtain a polysiloxane system, the polysiloxane system and the graphene and spherical alumina mixed powder are mixed and then vacuum stirred to obtain a graphene / spherical alumina / silica gel prepolymer;
[0010] (4) pouring the graphene / spherical alumina / silica gel prepolymer into a polytetrafluoroethylene mold and placing it in an oven for thermal curing to obtain a product;
[0011] (5) The product is subjected to hot pressing treatment to obtain a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material.
[0012] Furthermore, in step (1), the particle size of the nano-alumina in the nano-alumina ethanol dispersion is 40 nm, and the mass fraction is 20 wt%; the mass ratio of the graphene powder to the nano-alumina is 1:2-3; the amount of acetone and deionized water added is twice the mass of the graphene powder, and the mass ratio of acetone to deionized water is 2:1; the concentration of polyvinyl pyrrolidone in the mixed solution is 1.2 mg / mL.
[0013] Furthermore, in step (1), the stirring time is 60 minutes; the ultrasonic treatment time is 30 minutes, the ultrasonic frequency is 40KHz, and the power is 300W; the freeze-drying time is 48 hours, and the temperature is -60°C.
[0014] Furthermore, in step (2), the particle size distribution range of the mixed particle size spherical alumina is 3 to 70 μm; the mass ratio of the ethanol to deionized water is 9:1, 24 g of the mixed particle size spherical alumina is added to prepare a 50 mL solution; the silane coupling agent is KH-540, and the mass ratio of the silane coupling agent to the spherical alumina is 0.2 to 0.5:100.
[0015] Furthermore, in step (2), the constant temperature is 50° C.; the stirring time is 3 h; the ultrasonic treatment time is 30 min, the ultrasonic frequency is 40 KHz, and the power is 300 W.
[0016] Furthermore, in step (3), the mass fraction of the graphene powder loaded with nano-alumina is 3-15wt% of the graphene / spherical alumina / silica gel prepolymer, and the mass fraction of the modified spherical alumina powder is 40-60wt% of the graphene / spherical alumina / silica gel prepolymer.
[0017] Furthermore, in step (3), the viscosity of the vinyl-terminated polydimethylsiloxane is in the range of 500 to 30,000 mPa·s, and the content is 80 to 90 wt% of the polysiloxane system; the methyl hydrogen-containing silicone oil is a pendant hydrogen silicone oil and a terminal hydrogen silicone oil, wherein the content of the pendant hydrogen silicone oil is 5 to 11 wt% of the polysiloxane system, and the content of the terminal hydrogen silicone oil is 0.04 to 0.25 wt% of the polysiloxane system; the catalyst is selected from Castor The platinum catalyst has a content of 0.05-1.2wt% of the polysiloxane system, and the effective platinum concentration is 0.5-1.0wt% of the Custer platinum catalyst; the inhibitor is 1-ethynyl cyclohexanol, and the content is 0.01-0.5wt% of the sum of the masses of the terminal vinyl polydimethylsiloxane, the side hydrogen silicone oil and the terminal hydrogen silicone oil, and the total added amount of the terminal vinyl polydimethylsiloxane, the methyl hydrogen silicone oil, the catalyst and the inhibitor is 100wt%.
[0018] Furthermore, in step (3), the vacuum stirring time is 30 minutes and the rotation speed is 800 r / min.
[0019] Furthermore, in step (4), the thermal curing temperature is 80° C. and the time is 3 hours.
[0020] Furthermore, in step (5), the temperature of the hot pressing treatment is 120° C., the pressure is 30 MPa, and the time is 10 min.
[0021] The present invention provides a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material, which has the following beneficial effects:
[0022] 1. This preparation method forms a unique wrinkle structure by bonding graphene flakes to spherical alumina, which improves the graphene orientation in the vertical direction, is conducive to forming a continuous heat conduction path, and thus improves the thermal conductivity of the material. The obtained high-performance modified spherical alumina / wrinkle structure graphene / polysiloxane composite thermal conductive interface material has an in-plane thermal conductivity of up to 13.2 W / mK and an out-of-plane thermal conductivity of up to 3.063 W / mK.
[0023] 2. The preparation method modifies graphene and spherical alumina respectively, thereby improving the dispersibility of the thermal conductive filler in the polysiloxane system, reducing the agglomeration in the polymer matrix, and facilitating the formation of a continuous thermal conductive path, thereby improving the thermal conductivity of the material;
[0024] 3. This preparation method uses a blending casting and hot pressing process. This method is simple and controllable, low-cost, easy to mass-produce, and can be customized to the required shape according to different molds. It is widely used in the field of high-power electronic devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a schematic structural diagram of a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material prepared by a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material described in the present invention.
[0026] Among them, 1 is modified spherical alumina; 2 is graphene loaded with nano-alumina; 3. polysiloxane. DETAILED DESCRIPTION
[0027] The present invention provides a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material, comprising the steps of:
[0028] 1. Preparation of graphene powder loaded with nano-alumina: Weigh an appropriate amount of graphene powder, add nano-alumina ethanol dispersion, acetone, deionized water and polyvinyl pyrrolidone, stir for 60 minutes, ultrasonically treat for 30 minutes at an ultrasonic frequency of 40KHz and a power of 300W to make a uniform mixed solution, freeze and freeze-dry at a temperature of -60°C for 48 hours for use. Among them, the particle size of nano-alumina in the nano-alumina ethanol dispersion is 40nm, and the mass fraction is 20wt%; the mass ratio of the added graphene powder to the nano-alumina is 1:2-3; the amount of acetone and deionized water added is twice the mass of the graphene powder, and the mass ratio of acetone and deionized water is 2:1; the concentration of polyvinyl pyrrolidone in the mixed solution is 1.2mg / mL.
[0029] 2. Preparation of modified spherical alumina powder: Mix spherical alumina of mixed particle size, add deionized water and ethanol, and then add silane coupling agent to treat the surface of alumina, adjust pH to weak acidity with glacial acetic acid, stir at a constant temperature of 50°C for 3h, ultrasonically treat for 30min under the conditions of ultrasonic frequency of 40KHz and power of 300W, vacuum filter, wash with deionized water and dry for use. Among them, the particle size distribution range of spherical alumina is 3-70μm; the mass ratio of ethanol to deionized water is 9:1, 24g of spherical alumina of mixed particle size is added to prepare 50mL of solution; the silane coupling agent is KH-540, and its amount is 0.2-0.5:100 with the mass ratio of spherical alumina.
[0030] 3. Preparation of graphene / spherical alumina / silica gel prepolymer: The graphene powder loaded with nano-alumina and the modified spherical alumina powder are uniformly mixed to obtain a graphene and spherical alumina mixed powder. Appropriate amounts of vinyl-terminated polydimethylsiloxane, methyl hydrogen-containing silicone oil (side hydrogen silicone oil and end hydrogen silicone oil), catalyst and inhibitor are weighed and mixed to obtain a polysiloxane system, and the polysiloxane system and the graphene and spherical alumina mixed powder are mixed and stirred in vacuum at a speed of 800 r / min for 30 minutes to obtain a graphene / spherical alumina / silica gel prepolymer. The total amount of vinyl-terminated polydimethylsiloxane, methyl hydrogen silicone oil, catalyst and inhibitor added is 100wt%, the viscosity of vinyl-terminated polydimethylsiloxane is in the range of 500 to 30000mPa·s, and its content is 80 to 90wt% of the polysiloxane system; the content of pendant hydrogen silicone oil is 5 to 11wt% of the polysiloxane system; the content of hydrogen-terminated silicone oil is 0.04 to 0.25wt% of the polysiloxane system; the catalyst is selected from Custer platinum catalyst, and its content is 0.0 The catalyst comprises a 1-ethynylcyclohexanol and a 2-hydroxy-2-nitrogen-2-ol (2-hydroxy-2-nitrogen-2-ol) catalyst. ... 1-ethynylcyclohexanol and the 2-hydroxy-2-nitrogen-2-ol (2-hydroxy-2-nitrogen-2-ol) catalyst. The 1-ethynylcyclohexanol and the 2-hydroxy-2-nitrogen-2-ol (2-hydroxy-2-nitrogen-2-ol) catalyst comprises a 1-ethynylcyclohexanol and a 2-hydroxy-2-nitrogen-2-ol (2-hydroxy-2-nitrogen-2-ol) catalyst. The 1-ethynylcyclohexanol and the 2-hydroxy-2-nitrogen-2-ol (2-hydroxy-2-nitrogen-2-ol) catalyst comprises a 1-ethynylcyclohexanol and a 2-hydroxy-2-nitrogen-2-ol (2-hydroxy-2-nitrogen-2-ol) catalyst. The 1-ethynylcyclohexanol and the 2-hydroxy-2-nitrogen-2-ol (2-hydroxy-2-nitrogen-2-ol) catalyst comprises a 1-ethynylcyclohexanol and a 2-hydroxy-2-nitrogen-2-ol (2-hydroxy-2-nitrogen-2-ol) catalyst.
[0031] 4. Pour the graphene / spherical alumina / silica gel prepolymer into a polytetrafluoroethylene mold, place it in an oven, and perform thermal curing at a temperature of 80° C. for 3 h to obtain a product.
[0032] 5. The completely cured product was hot-pressed at a temperature of 120°C and a pressure of 30 MPa for 10 min to finally obtain a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material. For its specific structure, please refer to Figure 1 The modified spherical alumina 1, the graphene loaded with nano-alumina 2 and the polysiloxane 3 are tightly combined, and the graphene loaded with nano-alumina 2 is attached to the edge of the modified spherical alumina 1 to form a continuous heat conduction path with a pleated structure in the horizontal and vertical directions.
[0033] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the technical solutions of the present invention are further described below in conjunction with embodiments. However, the present invention is not limited to the embodiments listed, and should also include any other known changes within the scope of the rights claimed by the present invention.
[0034] The term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0035] Example 1
[0036] This embodiment demonstrates a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to the following steps:
[0037] S1. Preparation of graphene powder loaded with nano-alumina: Weigh 2g of graphene powder with a mass ratio of graphene to nano-alumina of 1:2, mix 20g of nano-alumina ethanol dispersion (20wt%), acetone, and deionized water to make a 50mL solution, and add 60mg of polyvinyl pyrrolidone. After stirring for 60min, treat with ultrasound at an ultrasonic frequency of 40KHz and a power of 300W for 30min to make a uniform mixed solution, freeze it, and freeze-dry it at -60℃ for 48h. Prepare several portions of mixed powder according to this ratio for use.
[0038] S2. Preparation of modified spherical alumina powder: Weigh 24 g of spherical alumina of mixed particle size (3 μm: 5 μm: 10 μm: 40 μm: 70 μm = 1:1:2:2:2), add deionized water and ethanol (mass ratio 1:9), and then add 120 mg of silane coupling agent to prepare 50 mL of mixed solution, adjust the pH to weak acidity (<7) with glacial acetic acid, stir for 3 h at a constant temperature, and perform ultrasonic treatment for 30 min at an ultrasonic frequency of 40 kHz and a power of 300 W. Then perform vacuum filtration, wash with deionized water, and dry for use.
[0039] S3, preparation of graphene / spherical alumina / silica gel prepolymer: weigh 1.2g of graphene powder loaded with nano-alumina, 16g of modified spherical alumina powder and mix them evenly to obtain a graphene and spherical alumina mixed powder. Weigh 22.8g of vinyl-terminated polydimethylsiloxane, side hydrogen silicone oil, hydrogen-terminated silicone oil, catalyst, and inhibitor mixture to obtain a polysiloxane system. Mix the graphene and spherical alumina mixed powder with the polysiloxane system and stir them in vacuum for 30min to obtain a graphene / spherical alumina / silica gel prepolymer.
[0040] S4. Pour the graphene / spherical alumina / silica gel prepolymer into a polytetrafluoroethylene mold and place it in an oven at 80°C for thermal curing for 3 hours.
[0041] S5. Hot-press the completely cured product at 120° C. and 30 MPa for 10 min to obtain the final composite thermal conductive interface material.
[0042] Example 2
[0043] This embodiment demonstrates a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to the following steps:
[0044] S1. Preparation of graphene powder loaded with nano-alumina: Weigh 2g of graphene powder with a mass ratio of graphene to nano-alumina of 1:3, mix 30g of nano-alumina ethanol dispersion (20wt%), acetone, and deionized water to make a 50mL solution, and add 60mg of polyvinyl pyrrolidone. After stirring for 60min, treat with ultrasound at an ultrasonic frequency of 40KHz and a power of 300W for 30min to make a uniform mixed solution, freeze it, and freeze-dry it at -60℃ for 48h. Prepare several portions of mixed powder according to this ratio for use.
[0045] S2. Preparation of modified spherical alumina powder: Weigh 24 g of spherical alumina of mixed particle size (3 μm: 5 μm: 10 μm: 40 μm: 70 μm = 1:1:2:2:2), add deionized water and ethanol (mass ratio 1:9), and then add 120 mg of silane coupling agent to prepare 50 mL of mixed solution, adjust the pH to weak acidity (<7) with glacial acetic acid, stir for 3 h at a constant temperature, and perform ultrasonic treatment for 30 min at an ultrasonic frequency of 40 kHz and a power of 300 W. Then perform vacuum filtration, wash with deionized water, and dry for use.
[0046] Steps S3 to S5 are the same as those in Example 1.
[0047] Example 3
[0048] This embodiment demonstrates a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to the following steps:
[0049] S1. Preparation of graphene powder loaded with nano-alumina: Weigh 2g of graphene powder with a mass ratio of graphene to nano-alumina of 1:3, mix 30g of nano-alumina ethanol dispersion (20wt%), acetone, and deionized water to make a 50mL solution, and add 60mg of polyvinyl pyrrolidone. After stirring for 60min, treat with ultrasound at an ultrasonic frequency of 40KHz and a power of 300W for 30min to make a uniform mixed solution, freeze it, and freeze-dry it at -60℃ for 48h. Prepare several portions of mixed powder according to this ratio for use.
[0050] S2. Preparation of modified spherical alumina powder: Weigh 24 g of spherical alumina of mixed particle size (3 μm: 5 μm: 10 μm: 40 μm: 70 μm = 1:1:2:2:2), add deionized water and ethanol (mass ratio 1:9), and then add 48 mg of silane coupling agent to prepare 50 mL of mixed solution, adjust the pH to weak acidity (<7) with glacial acetic acid, stir for 3 h at a constant temperature, and perform ultrasonic treatment for 30 min at an ultrasonic frequency of 40 kHz and a power of 300 W. Then perform vacuum filtration, wash with deionized water, and dry for use.
[0051] Steps S3 to S5 are the same as those in Example 1.
[0052] Example 4
[0053] This embodiment demonstrates a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to the following steps:
[0054] Steps S1 and S2 are the same as those in Example 2.
[0055] S3, preparation of graphene / spherical alumina / silica gel prepolymer: weigh 1.2g of graphene powder loaded with nano-alumina, 18g of modified spherical alumina powder and mix them evenly to obtain a graphene and spherical alumina mixed powder. Weigh 20.8g of vinyl-terminated polydimethylsiloxane, side hydrogen silicone oil, hydrogen-terminated silicone oil, catalyst, and inhibitor mixture to obtain a polysiloxane system. Mix the graphene and spherical alumina mixed powder with the polysiloxane system and stir them in vacuum for 30min to obtain a graphene / spherical alumina / silica gel prepolymer.
[0056] S4. Pour the graphene / spherical alumina / silica gel prepolymer into a polytetrafluoroethylene mold and place it in an oven at 80°C for thermal curing for 3 hours.
[0057] S5. Hot-press the completely cured product at 120° C. and 30 MPa for 10 min to obtain the final composite thermal conductive interface material.
[0058] Example 5
[0059] This embodiment demonstrates a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to the following steps:
[0060] Steps S1 and S2 are the same as those in Example 2.
[0061] S3, preparation of graphene / spherical alumina / silica gel prepolymer: weigh 2.4g of graphene powder loaded with nano-alumina, and mix 18g of modified spherical alumina powder evenly to obtain a graphene and spherical alumina mixed powder. Weigh 19.6g of vinyl-terminated polydimethylsiloxane, side hydrogen silicone oil, hydrogen-terminated silicone oil, catalyst, and inhibitor mixture to obtain a polysiloxane system. Mix the graphene and spherical alumina mixed powder with the polysiloxane system and stir under vacuum for 30min to obtain a graphene / spherical alumina / silica gel prepolymer.
[0062] S4. Pour the graphene / spherical alumina / silica gel prepolymer into a polytetrafluoroethylene mold and place it in an oven at 80°C for thermal curing for 3 hours.
[0063] S5. Hot-press the completely cured product at 120° C. and 30 MPa for 10 min to obtain the final composite thermal conductive interface material.
[0064] Example 6
[0065] This embodiment demonstrates a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to the following steps:
[0066] Steps S1 and S2 are the same as those in Example 2.
[0067] S3, preparation of graphene / spherical alumina / silica gel prepolymer: weigh 4.8g of graphene powder loaded with nano-alumina, and mix 18g of modified spherical alumina powder evenly to obtain a graphene and spherical alumina mixed powder. Weigh 17.2g of vinyl-terminated polydimethylsiloxane, side hydrogen silicone oil, hydrogen-terminated silicone oil, catalyst, and inhibitor mixture to obtain a polysiloxane system. Mix the graphene and spherical alumina mixed powder with the polysiloxane system and stir in vacuum for 30min to obtain a graphene / spherical alumina / silica gel prepolymer.
[0068] S4. Pour the graphene / spherical alumina / silica gel prepolymer into a polytetrafluoroethylene mold and place it in an oven at 80°C for thermal curing for 3 hours.
[0069] S5. Hot-press the completely cured product at 120° C. and 30 MPa for 10 min to obtain the final composite thermal conductive interface material.
[0070] Example 7
[0071] This embodiment demonstrates a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to the following steps:
[0072] Steps S1 and S2 are the same as those in Example 2.
[0073] S3, preparation of graphene / spherical alumina / silica gel prepolymer: weigh 2.4g of graphene powder loaded with nano-alumina, and mix 20g of modified spherical alumina powder evenly to obtain a graphene and spherical alumina mixed powder. Weigh 17.6g of vinyl-terminated polydimethylsiloxane, side hydrogen silicone oil, hydrogen-terminated silicone oil, catalyst, and inhibitor mixture to obtain a polysiloxane system. Mix the graphene and spherical alumina mixed powder with the polysiloxane system and stir under vacuum for 30min to obtain a graphene / spherical alumina silica gel prepolymer.
[0074] S4. Pour the graphene / spherical alumina / silica gel prepolymer into a polytetrafluoroethylene mold and place it in an oven at 80°C for thermal curing for 3 hours.
[0075] S5. Hot-press the completely cured product at 120° C. and 30 MPa for 10 min to obtain the final composite thermal conductive interface material.
[0076] Example 8
[0077] This embodiment demonstrates a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to the following steps:
[0078] Steps S1 and S2 are the same as those in Example 2.
[0079] S3, preparation of graphene / spherical alumina / silica gel prepolymer: weigh 4.8g of graphene powder loaded with nano-alumina, and mix 20g of modified spherical alumina powder evenly to obtain a graphene and spherical alumina mixed powder. Weigh 15.2g of vinyl-terminated polydimethylsiloxane, side hydrogen silicone oil, hydrogen-terminated silicone oil, catalyst, and inhibitor mixture to obtain a polysiloxane system. Mix the graphene and spherical alumina mixed powder with the polysiloxane system and stir under vacuum for 30min to obtain a graphene / spherical alumina silica gel prepolymer.
[0080] S4. Pour the graphene / spherical alumina silica gel prepolymer into a polytetrafluoroethylene mold and place it in an oven at 80°C for thermal curing for 3 hours.
[0081] S5. Hot-press the completely cured product at 120° C. and 30 MPa for 10 min to obtain the final composite thermal conductive interface material.
[0082] Example 9
[0083] This embodiment demonstrates a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to the following steps:
[0084] S1. Preparation of graphene powder loaded with nano-alumina: Weigh 2g of graphene powder with a standard of graphene: nano-alumina mass ratio of 1:3, mix 30g of nano-alumina ethanol dispersion (20wt%), acetone, and deionized water to make a 50mL solution, and add 60mg of polyvinyl pyrrolidone. After stirring for 60min, ultrasonic treatment is performed at an ultrasonic frequency of 40KHz and a power of 300W for 30min to prepare a uniform mixed solution, which is then frozen and freeze-dried at -60°C for 48h. Several portions of mixed powder are prepared according to this ratio for standby use.
[0085] S2. Preparation of modified spherical alumina powder: Weigh 24 g of spherical alumina (3 μm), add deionized water and ethanol (mass ratio 1:9), and then add 120 mg of silane coupling agent to prepare 50 mL of mixed solution, adjust the pH to weak acidity (<7) with glacial acetic acid, stir for 3 h at a constant temperature, and perform ultrasonic treatment for 30 min at an ultrasonic frequency of 40 kHz and a power of 300 W. Then perform vacuum filtration, wash with deionized water, and dry for use.
[0086] S3, preparation of graphene / spherical alumina / silica gel prepolymer: weigh 4.8g of graphene powder loaded with nano-alumina, and mix 20g of modified spherical alumina powder evenly to obtain a graphene and spherical alumina mixed powder. Weigh 15.2g of vinyl-terminated polydimethylsiloxane, side hydrogen silicone oil, hydrogen-terminated silicone oil, catalyst, and inhibitor mixture to obtain a polysiloxane system. Mix the graphene and spherical alumina mixed powder with the polysiloxane system and stir under vacuum for 30min to obtain a graphene / spherical alumina silica gel prepolymer.
[0087] S4. Pour the graphene / spherical alumina / silica gel prepolymer into a polytetrafluoroethylene mold and place it in an oven at 80°C for thermal curing for 3 hours.
[0088] S5. Hot-press the completely cured product at 120° C. and 30 MPa for 10 min to obtain the final composite thermal conductive interface material.
[0089] Example 10
[0090] This embodiment demonstrates a method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to the following steps:
[0091] S1. Preparation of graphene powder loaded with nano-alumina: Weigh 2g of graphene powder with a mass ratio of graphene to nano-alumina of 1:3, mix 30g of nano-alumina ethanol dispersion (20wt%), acetone, and deionized water to make a 50mL solution, and add 60mg of polyvinyl pyrrolidone. After stirring for 60min, treat with ultrasound at an ultrasonic frequency of 40KHz and a power of 300W for 30min to make a uniform mixed solution, freeze it, and freeze-dry it at -60℃ for 48h. Prepare several portions of mixed powder according to this ratio for use.
[0092] S2. Preparation of modified spherical alumina powder: Weigh 24 g of spherical alumina (70 μm), add deionized water and ethanol (mass ratio 1:9), and then add 120 mg of silane coupling agent to prepare 50 mL of mixed solution, adjust the pH to weak acidity (<7) with glacial acetic acid, stir for 3 h at a constant temperature, and perform ultrasonic treatment for 30 min at an ultrasonic frequency of 40 kHz and a power of 300 W. Then perform vacuum filtration, wash with deionized water, and dry for use.
[0093] S3, preparation of graphene / spherical alumina / silica gel prepolymer: weigh 4.8g of graphene powder loaded with nano-alumina, 20g of modified spherical alumina powder, and obtain a mixed powder of graphene and spherical alumina. Weigh 15.2g of vinyl-terminated polydimethylsiloxane, side hydrogen silicone oil, hydrogen-terminated silicone oil, catalyst, and inhibitor mixture to obtain a polysiloxane system. Mix the graphene and spherical alumina mixed powder with the polysiloxane system and stir under vacuum for 30min to obtain a graphene / spherical alumina / silica gel prepolymer.
[0094] S4. Pour the graphene / spherical alumina / silica gel prepolymer into a polytetrafluoroethylene mold and place it in an oven at 80°C for thermal curing for 3 hours.
[0095] S5. Hot-press the completely cured product at 120° C. and 30 MPa for 10 min to obtain the final composite thermal conductive interface material.
[0096] Embodiment 11
[0097] Steps S1 and S2 are the same as those in Example 2.
[0098] S3, preparation of graphene / spherical alumina / silica gel prepolymer: weigh 6g of graphene powder loaded with nano-alumina, and mix 20g of modified spherical alumina powder evenly to obtain a graphene and spherical alumina mixed powder. Weigh 14g of vinyl-terminated polydimethylsiloxane, side hydrogen silicone oil, hydrogen-terminated silicone oil, catalyst, and inhibitor mixture to obtain a polysiloxane system. Mix the graphene and spherical alumina mixed powder with the polysiloxane system and stir in vacuum for 30min to obtain a graphene / spherical alumina silica gel prepolymer.
[0099] S4. Pour the graphene / spherical alumina silica gel prepolymer into a polytetrafluoroethylene mold and place it in an oven at 80°C for thermal curing for 3 hours.
[0100] S5. Hot-press the completely cured product at 120° C. and 30 MPa for 10 min to obtain the final composite thermal conductive interface material.
[0101] Example 12
[0102] Steps S1 and S2 are the same as those in Example 2.
[0103] S3, preparation of graphene / spherical alumina / silica gel prepolymer: weigh 4.8g of graphene powder loaded with nano-alumina, and mix 24g of modified spherical alumina powder evenly to obtain a graphene and spherical alumina mixed powder. Weigh 11.2g of vinyl-terminated polydimethylsiloxane, side hydrogen silicone oil, hydrogen-terminated silicone oil, catalyst, and inhibitor mixture to obtain a polysiloxane system. Mix the graphene and spherical alumina mixed powder with the polysiloxane system and stir under vacuum for 30min to obtain a graphene / spherical alumina silica gel prepolymer.
[0104] S4. Pour the graphene / spherical alumina silica gel prepolymer into a polytetrafluoroethylene mold and place it in an oven at 80°C for thermal curing for 3 hours.
[0105] S5. Hot-press the completely cured product at 120° C. and 30 MPa for 10 min to obtain the final composite thermal conductive interface material.
[0106] Comparative Example 1
[0107] The preparation method of this comparative example is different from that of Example 8 only in that modified spherical alumina is not added in step S3.
[0108] Comparative Example 2
[0109] The preparation method of this comparative example is different from that of Example 8 only in that the hot pressing treatment in step S5 is not performed.
[0110] The thermal interface materials obtained in Examples 1 to 12 and Comparative Examples 1 to 2 were subjected to performance tests, wherein the density test was measured using a balance method, the test was conducted using the GB4472-84 standard, the sample was a square sample with a thickness of 3 mm and a side length of 50 mm, the test was repeated three times, and the average value was taken; the thermal conductivity was determined using a guarded hot plate method thermal conductivity instrument, the steady-state test was conducted using the ASTM-D5470 standard, the sample of the thermal interface material was a circular sample with a thickness of 0.5 mm and a diameter of 20 mm, the test was repeated three times, and the average value was taken; the test results are shown in Table 1 below:
[0111]
[0112]
[0113] It can be seen from Table 1 that, compared with Example 1, Example 2 increases the content of nano-alumina loaded on graphene. According to the test results, the thermal conductivity coefficients inside and outside the plane are slightly improved; compared with Example 2, Example 3 reduces the content of silane coupling agent KH-540. According to the test results, the thermal conductivity coefficients inside and outside the plane are slightly decreased. This is because the content of silane coupling agent is insufficient and the spherical alumina is unevenly dispersed in the polymer matrix; compared with Example 2, Example 4 increases the content of modified spherical alumina. According to the test results, after increasing the mass of modified spherical alumina, the out-of-plane thermal conductivity is improved, but the in-plane thermal conductivity is decreased.Compared with Example 4, Example 5 increases the content of graphene loaded with nano-alumina. According to the analysis of the test results, after the concentration of graphene loaded with nano-alumina is increased, the thermal conductivity of the composite material inside and outside the plane is significantly improved; Compared with Example 5, Example 6 further increases the content of graphene loaded with nano-alumina. According to the analysis of the test results, after the concentration of graphene loaded with nano-alumina is increased within a certain range, the thermal conductivity of the composite material inside and outside the plane is significantly improved; Compared with Example 5, Example 7 increases the concentration of modified spherical alumina. According to the analysis of the test results, the thermal conductivity in the vertical direction (out of the plane) is significantly increased, but the thermal conductivity in the plane is decreased; Compared with Example 7, Example 8 further increases the content of graphene loaded with nano-alumina. According to the analysis of the test results, the thermal conductivity in the vertical direction (out of the plane) is significantly increased, but the thermal conductivity in the plane is decreased. The graphene content of the loaded nano-alumina was further increased. According to the test results, the thermal conductivity both in and out of the plane was significantly improved. At this time, the synergistic effect of spherical alumina and flaky graphene was better. Compared with Example 8, Example 9 did not use modified spherical alumina with mixed particle sizes, and only modified spherical alumina with a particle size of 3 μm was added. According to the test results, the out-of-plane thermal conductivity was significantly reduced. This is because the spherical alumina with a small particle size cannot attach to a large number of graphene sheets, and the wrinkle structure is not obvious. Compared with Example 8, Example 10 only added modified spherical alumina with a particle size of 70 μm. According to the test results, the out-of-plane thermal conductivity is higher, but the in-plane thermal conductivity is significantly reduced. This is because the spherical alumina with a large particle size can attach to a large The amount of graphene sheets is increased to form an obvious wrinkle structure, but a large amount of large-particle spherical alumina easily destroys the thermal conductivity path of the graphene in the in-plane direction; compared with Example 8, Example 11 further increases the content of graphene loaded with nano-alumina. According to the test results, the thermal conductivity coefficients in and out of the plane are slightly reduced; compared with Example 8, Example 12 further increases the content of modified spherical alumina. According to the test results, the in-plane thermal conductivity coefficient is significantly reduced, and the excessive spherical alumina hinders the continuity of the thermal conductivity path of the graphene sheet; compared with Example 8, Comparative Example 1, according to the test results, the out-of-plane thermal conductivity coefficient is significantly reduced. This is because no modified spherical alumina is used in the preparation, so that the graphene sheet does not form a wrinkle structure. The lack of an out-of-plane heat conduction path reduces the thermal conductivity of the composite material. Compared with Example 8, according to the test results, the thermal conductivity of Comparative Example 2 is reduced, indicating that the hot pressing step can make the polymer matrix and the thermally conductive filler inside the composite material more closely combined, reduce the interfacial thermal resistance between fillers and fillers, and between fillers and the matrix, so that the thermal conductivity of the composite material is further improved. It should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention is described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material, characterized in that: The method includes: (1) Preparation of graphene powder loaded with nano-alumina: Weigh graphene powder, add nano-alumina ethanol dispersion, acetone, deionized water and polyvinyl pyrrolidone, stir thoroughly, ultrasonicate to form a uniform mixed solution, freeze and freeze-dry to obtain graphene powder loaded with nano-alumina, wherein the particle size of nano-alumina in the nano-alumina ethanol dispersion is 40 nm, and the mass fraction is 20 wt %; the mass ratio of the graphene powder to the nano-alumina is 1:2-3; the amount of acetone and deionized water added is twice the mass of the graphene powder, and the mass ratio of acetone to deionized water is 2:1; the concentration of polyvinyl pyrrolidone in the mixed solution is 1.2 mg / mL; (2) Preparation of modified spherical alumina powder: spherical alumina of mixed particle sizes are mixed, deionized water and ethanol are added, and then a silane coupling agent is added to treat the surface of the spherical alumina, the pH is adjusted to be weakly acidic by glacial acetic acid, the mixture is fully stirred, ultrasonically treated, and vacuum filtered at a constant temperature, and then washed with deionized water and dried to obtain modified spherical alumina powder, wherein the composition of the spherical alumina of mixed particle sizes is 3 μm: 5 μm: 10 μm: 40 μm: 70 μm = 1:1:2:2:2; the mass ratio of the ethanol to the deionized water is 9:1, 24 g of the spherical alumina of mixed particle sizes is added, and a 50 mL solution is prepared; the silane coupling agent is KH-540, and the mass ratio of the silane coupling agent to the spherical alumina is 0.2-0.5:100; (3) Preparation of graphene / spherical alumina / silica gel prepolymer: the graphene powder loaded with nano-alumina is uniformly mixed with the modified spherical alumina powder to obtain a graphene and spherical alumina mixed powder, vinyl-terminated polydimethylsiloxane, methyl hydrogen silicone oil, a catalyst and an inhibitor are weighed to obtain a polysiloxane system, the polysiloxane system and the graphene and spherical alumina mixed powder are mixed and then vacuum stirred to obtain a graphene / spherical alumina / silica gel prepolymer; (4) pouring the graphene / spherical alumina / silica gel prepolymer into a polytetrafluoroethylene mold and placing it in an oven for thermal curing to obtain a product; (5) The product is subjected to hot pressing treatment to obtain a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material.
2. The method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to claim 1, characterized in that: In step (1), the stirring time is 60 minutes; the ultrasonic treatment time is 30 minutes, the ultrasonic frequency is 40KHz, and the power is 300W; the freeze-drying time is 48 hours, and the temperature is -60°C.
3. The method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to claim 1, characterized in that: In step (2), the constant temperature is 50° C.; the stirring time is 3 h; the ultrasonic treatment time is 30 min, the ultrasonic frequency is 40 KHz, and the power is 300 W.
4. The method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to claim 1, characterized in that: In step (3), the mass fraction of the graphene powder loaded with nano-alumina is 3-15wt% of the graphene / spherical alumina / silica gel prepolymer, and the mass fraction of the modified spherical alumina powder is 40-60wt% of the graphene / spherical alumina / silica gel prepolymer.
5. The method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to claim 1, characterized in that: In step (3), the viscosity of the vinyl-terminated polydimethylsiloxane is in the range of 500 to 30,000 mPa·s, and its content is 80 to 90 wt% of the polysiloxane system; the methyl hydrogen-containing silicone oil is pendant hydrogen silicone oil and terminal hydrogen silicone oil, wherein the content of the pendant hydrogen silicone oil is 5 to 11 wt% of the polysiloxane system, and the content of the terminal hydrogen silicone oil is 0.04 to 0.25 wt% of the polysiloxane system; the catalyst is selected from a Custer platinum catalyst, and its content is 0.05 to 1.2 wt% of the polysiloxane system, and its effective platinum concentration is 0.5 to 1.0 wt% of the Custer platinum catalyst; the inhibitor is 1-ethynyl cyclohexanol, and its content is 0.01 to 0.5 wt% of the sum of the masses of the vinyl-terminated polydimethylsiloxane, pendant hydrogen silicone oil and terminal hydrogen silicone oil, and the total amount of the vinyl-terminated polydimethylsiloxane, methyl hydrogen-containing silicone oil, catalyst and inhibitor added is 100 wt%.
6. The method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to claim 1, characterized in that: In step (3), the vacuum stirring time is 30 minutes and the rotation speed is 800 r / min.
7. The method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to claim 1, characterized in that: In step (4), the thermal curing temperature is 80° C. and the time is 3 hours.
8. The method for preparing a modified spherical alumina / corrugated graphene / polysiloxane composite thermal conductive interface material according to claim 1, characterized in that: In step (5), the temperature of the hot pressing treatment is 120° C., the pressure is 30 MPa, and the time is 10 min.
Citation Information
Patent Citations
Graphene-containing silicone rubber composite material with high thermal conductivity and preparation method thereof
CN103627179A
Nanometer alpha-aluminum oxide loaded thermal reduction graphene and preparation method thereof, and high-thermal-conductivity electrical insulation elastomer thermal interface material
CN111171381A
Silicone rubber high-heat-conducting material
CN112080149A
Heat-conducting film composite material and preparation method thereof
CN113278406A
Carbon fiber heat-conducting phase-change composite material and preparation method therefor
WO2024008020A1
Cited By
Preparation method of reaction type graphene reinforced spherical core-shell structure Al2O3 (at) Al heat conduction interface material
CN120464207A