A method for reducing adhesion of ultra-high molecular weight polyethylene fibers

By using a combined method of high-pressure hot air and an ultrasonic functional water bath after the gelatin silk extraction, the problem of fiber adhesion of ultra-high molecular weight polyethylene fiber was solved, the mechanical properties and production efficiency of the fiber were improved, and the process flow was simplified.

CN118127650BActive Publication Date: 2024-10-29NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410221072.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-28
Publication Date
2024-10-29
Estimated Expiration
2044-02-28

AI Technical Summary

Technical Problem

Ultra-high molecular weight polyethylene fibers are prone to fiber adhesion during the gel spinning process, which affects the spreading and weaving quality of the fibers. Existing methods are difficult to effectively solve and increase production complexity and energy consumption.

Method used

After the gel filament is extracted, high-pressure hot air is used to purge and quickly enter a constant-temperature water bath with ultrasonic function for heat drawing. Through the combination of ultrasonic waves and hot water, the extraction agent is quickly evaporated, reducing the adhesion between fibers, and Super hot drawing is carried out through a 4-stage hot box to optimize fiber orientation and mechanical properties.

Benefits of technology

It significantly reduces the adhesion rate of the fiber, increases the breaking strength and initial modulus of the fiber, simplifies the production process, reduces energy consumption, and improves the uniformity and mechanical properties of the fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118127650B_ABST
    Figure CN118127650B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for reducing the adhesion of ultra-high molecular weight polyethylene fibers, comprising: blowing high-pressure hot air through the extracted fiber bundle, passing it into a water bath thermostat with an ultrasonic function, the high-pressure hot air temperature is 40-100°C, the ultrasonic power is ≥4000W, the water bath temperature is 50-99°C, the effective distance of the fiber bundle in the water bath is ≥4 meters, and the draft ratio of the fiber bundle in the water bath is 1.2-5.0; after the fiber bundle passes through the water bath thermostat to quickly remove the extractant and perform heat drawing, it is blown with compressed air to remove the moisture on the surface, and then passed through a hot box for super-multiple heat drawing to obtain ultra-high molecular weight polyethylene fibers. The present invention provides a constant temperature water bath with a high-power ultrasonic function after extraction, and quickly passes the extracted fiber into the constant temperature water bath, so that the extractant on the fiber surface evaporates quickly, and the ultra-high molecular weight polyethylene molecular chains of small molecules in adjacent fibers fail to migrate to the fiber surface to generate entanglement, thereby greatly reducing the adhesion of the fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of high-performance fiber preparation, and in particular relates to a method for reducing adhesion of ultra-high molecular weight polyethylene fibers. Background Art

[0002] Ultra-high molecular weight polyethylene fiber, also known as high-strength high-modulus polyethylene fiber, has a linear straight chain structure composed of simple methylene groups in its macromolecular chain, with a fiber orientation of more than 95% and a crystallinity of more than 90%. It has excellent properties such as low density, high strength, corrosion resistance, and impact resistance. It is currently the fiber with the highest specific strength and specific modulus in the world. Ultra-high molecular weight polyethylene fiber has superior properties that other fibers cannot match, and is an ideal material for making soft bulletproof vests, stab-proof clothing, bulletproof helmets, radar covers, bulletproof armor, ships and ocean-going ship cables, aerospace structural parts, fishing lines, surgical sutures, etc.

[0003] At present, ultra-high molecular weight polyethylene fibers are mainly produced by gel spinning-super-stretching technology. After ultra-high molecular weight polyethylene is dissolved in a solvent, its macromolecules are in a low entanglement state. The gel fibers obtained after spinning are extracted, dried, and stretched at high times to straighten the flexible macromolecules of the folded chain, and are highly oriented and crystallized along the fiber axis to obtain high-strength and high-modulus ultra-high molecular weight polyethylene fibers. It is found through existing technology that after ultra-high molecular weight polyethylene gel fibers are extracted and dried, the fibers show different degrees of adhesion. The adhesion between fibers will affect the use of downstream markets to a certain extent, affect the spreading of fibers in the process of making composite materials, and make soft bulletproof vests, fishing lines, surgical sutures and other woven products. When making woven products, it will make the fiber flexibility worse, affect the weaving of the fiber, and lead to a decrease in product quality.

[0004] At present, a Chinese invention patent with application number 202111611626.2 discloses a method for reducing the parallelization rate of ultra-high molecular weight polyethylene fibers in the manufacturing process. In the ultra-high molecular weight polyethylene gel spinning process, the parallelization rate of ultra-high molecular weight polyethylene fibers is reduced by selecting suitable raw material components and increasing multiple cold drawing; however, the selected spinning solution concentration is relatively high. In the existing ultra-high molecular weight polyethylene fiber production process, the spinning solution concentration of ultra-high strength ultra-high molecular weight polyethylene fibers and fine denier ultra-high molecular weight polyethylene fibers is mostly ≤8%, so it is difficult to be widely used in the existing ultra-high molecular weight polyethylene fiber production process. At the same time, multiple increases in cold drawing also make the production process more complicated, affecting production efficiency.

[0005] Therefore, fundamentally solving the problem of fiber adhesion during the ultra-high molecular weight polyethylene fiber gel spinning process is a technical problem that needs to be solved urgently in this field. Summary of the invention

[0006] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0007] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0008] Therefore, the object of the present invention is to overcome the deficiencies in the prior art and provide a method for reducing adhesion of ultra-high molecular weight polyethylene fibers.

[0009] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for reducing adhesion of ultra-high molecular weight polyethylene fibers, comprising:

[0010] After the primary jelly silk is extracted in an extraction tank, a fiber bundle containing a large amount of extractant inside and on the surface is obtained;

[0011] The fiber bundle obtained after extraction is blown with high-pressure hot air, and then quickly passed into a water bath thermostatic tank with ultrasonic function, the high-pressure hot air temperature is 40-100°C, the ultrasonic power is ≥4000W, the water bath temperature is 50-99°C, the effective distance of the fiber bundle in the water bath is ≥4 meters, and the draft ratio of the fiber bundle in the water bath is 1.2-5.0;

[0012] The fiber tow passes through a water bath thermostatic tank to quickly remove the extractant and is heat-stretched, then is purged with compressed air to remove surface moisture, and then passes through a heat box for super-heat stretching to obtain ultra-high molecular weight polyethylene fibers.

[0013] As a preferred embodiment of the method of the present invention, the preparation method of the primary jelly silk comprises:

[0014] Ultra-high molecular weight polyethylene powder, spinning solvent and antioxidant are added to a high-speed mixer and mixed evenly, and then added to a feeding kettle, and then the feeding kettle is evacuated and nitrogen is passed through for three times to replace the air in the feeding kettle and the solution to obtain a spinning solution;

[0015] The obtained spinning solution is added to the feeding port of the twin-screw extruder, dissolved by the twin-screw extruder, quantitatively extruded by the metering pump, and then passed through the spinneret, nozzle drawing, coagulation bath, and the primary jelly yarn is obtained.

[0016] As a preferred embodiment of the method of the present invention, the coagulation bath is a mixture of water and a nonionic surfactant, the nonionic surfactant is one or a mixture of NP-9, NP-10, and TX-10, the nonionic surfactant accounts for 0.01 to 0.15 wt% of the total mass of the coagulation bath, and the temperature of the coagulation bath is 0 to 15°C.

[0017] As a preferred embodiment of the method of the present invention, the molecular weight of the ultra-high molecular weight polyethylene powder is 5000000-9000000 g / mol, and the molecular weight distribution is 1.5-2.5; the bulk density of the ultra-high molecular weight polyethylene powder is 0.30-0.50 g / cm 3 .

[0018] As a preferred embodiment of the method of the present invention, the average particle size of the ultra-high molecular weight polyethylene powder is D≤80um and the particle size distribution is D±5um; the ultra-high molecular weight polyethylene powder accounts for 5-12wt% of the total mass of the mixed spinning solution.

[0019] As a preferred embodiment of the method of the present invention, the spinning solvent is one or more hydrocarbons, including one or more of decalin, tetralin, kerosene, and liquid paraffin.

[0020] As a preferred embodiment of the method of the present invention, the antioxidant is one or a mixture of phenolic antioxidants and phosphite antioxidants, including one or a mixture of tris[2,4-di-tert-butylphenyl]phosphite, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,6-di-tert-butyl-4-methylphenol, distearyl pentaerythritol diphosphite; the antioxidant is added in an amount of 0.1 to 1.0 wt% of the mass of the ultra-high molecular weight polyethylene powder.

[0021] As a preferred embodiment of the method of the present invention, wherein: the preparation of primary jelly silk, wherein:

[0022] Screw diameter 36-150mm, aspect ratio 45-65;

[0023] Screw speed: 400~1200RPM;

[0024] The temperature of the screw feeding section is 90-160°C, the temperature of the screw compression section is 160-180°C, and the temperature of the screw homogenization section is 170-180°C;

[0025] The number of holes of the spinneret is 2 to 2000, and the height from the spinneret to the surface of the coagulation bath is 1 to 15 cm.

[0026] As a preferred embodiment of the method of the present invention, the extractant is one or more combinations of xylene, dichloromethane, carbon tetrachloride, dichloroethane, n-hexane, gasoline, and hydrocarbon cleaning agents, and the extraction temperature is 20-50°C.

[0027] As a preferred embodiment of the method of the present invention, the super-multiple hot stretching is performed by a hot box, wherein a 4-stage hot box stretching is adopted, the effective heating length of each hot box is 4 meters, the internal temperature of the hot box is 100-150°C, and the total stretching multiple of the hot box is 15-40 times.

[0028] As a preferred embodiment of the method of the present invention, the adhesion rate of the ultra-high molecular weight polyethylene fiber is ≤3%, the fiber breaking strength is ≥42 cN / dtex, the initial modulus is ≥1800 cN / dtex, the molecular weight of the ultra-high molecular weight polyethylene fiber is ≥3500000 g / mol, and the molecular weight distribution is 2.0 to 3.5.

[0029] Beneficial effects of the present invention:

[0030] (1) The present invention proposes a method for reducing the adhesion of ultra-high molecular weight polyethylene fibers. After the primary jelly fibers are extracted, a constant temperature water bath with a high-power ultrasonic function is set. The extracted fibers are blown with high-pressure hot air and then quickly passed into a constant temperature water bath. A certain proportion of stretching is applied to the fibers so that the extractant on the fiber surface evaporates quickly after the extraction is completed. The small molecules of ultra-high molecular weight polyethylene in adjacent fibers cannot migrate to the fiber surface to generate entanglement, thereby greatly reducing the adhesion of the fibers.

[0031] (2) The present invention replaces the drying box in the existing process with a constant temperature water bath, which greatly improves the drying efficiency, reduces production energy consumption, and simplifies production equipment.

[0032] (3) The present invention performs heat stretching in a constant temperature water bath. During the stretching process, the fibers are completely immersed in hot water, so that the fibers are heated more evenly during the stretching process, and the fibers obtained after stretching have better uniformity.

[0033] (4) The present invention reduces the adhesion between fibers and reduces the stress concentration points in the fiber bundle, so that the breaking strength and initial modulus of the fibers are correspondingly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0035] Figure 1 It is a process system diagram in an embodiment of the present invention. DETAILED DESCRIPTION

[0036] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0037] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0038] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0039] The breaking strength and initial modulus test standard of the ultra-high molecular weight polyethylene fiber in the present invention is: GB / T19975-2005;

[0040] Molecular weight and distribution test standard of ultra-high molecular weight polyethylene powder and ultra-high molecular weight polyethylene fiber: ISO16014-4:2019;

[0041] Fiber adhesion (parallel yarn) rate test method: cut a uniform short piece of short yarn from a bundle of ultra-high molecular weight polyethylene fiber filaments to make a fiber sample to be tested, use a detection instrument to obtain an image of the fiber sample to be tested, and obtain the number of fibers in this bundle through manual or software analysis, and record its number as n. The number of spinneret holes for preparing this bundle of samples is recorded as F, and the fiber adhesion rate N = Fn / F×100%.

[0042] The raw materials in the present invention are all common commercially available products.

[0043] The process system diagram of the present invention is shown in Figure 1, including a feeding kettle 100, a twin screw 200, a metering pump 300, a spinning assembly 400, a coagulation bath 500, a wire barrel 600, an extraction tank 700, a constant temperature water bath 800 with ultrasonic function, a 4-stage hot box drawing device 900 and a wire winding device 1000; wherein, the constant temperature water bath 800 with ultrasonic function is provided with a high-pressure hot air blowing device 801 and a compressed air blowing device 802 in two sections, and the 4-stage hot box drawing device 900 includes a seven-roller drawing device 1 901, a hot box 1 902, a seven-roller drawing device 2 903, a hot box 2 904, a seven-roller drawing device 3 905, a hot box 3 906, a seven-roller drawing device 4 907, a hot box 4 908, and a seven-roller drawing device 5 909;

[0044] Specifically, the spinning solution is dissolved by the twin screw 200 from the feeding kettle 100, quantitatively extruded by the metering pump 300, and then passed through the spinneret assembly 400 and the coagulation bath 500 to obtain the primary jelly filaments; wherein the distance between the spinneret in the spinneret assembly and the coagulation bath is 1 to 15 cm, the coagulation bath is a non-ionic surfactant aqueous solution with a mass fraction of 0.01 to 0.15 wt%, and the coagulation bath temperature is 0 to 15°C;

[0045] After the raw gel fibers are extracted by the fiber storage barrel 600 and the extraction tank 700, and then blown with high-pressure hot air by the high-pressure hot air blowing device 801, the fibers are quickly passed into the constant temperature water bath 800 with ultrasonic function;

[0046] The fibers drawn out from the constant temperature water bath are blown by the compressed air blowing device 802 to remove the water on the fiber surface, and then drawn through a 4-stage hot box and collected to obtain ultra-high molecular weight polyethylene fibers.

[0047] Example 1

[0048] 20 kg of ultra-high molecular weight polyethylene powder with a molecular weight of 6500000 g / mol, 180 kg of tetralin, 50 g of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and 100 g of tris[2,4-di-tert-butylphenyl]phosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier, and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 10%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the molecular weight distribution of the ultra-high molecular weight polyethylene powder is 2.2, the bulk density is 0.42 g / cm3, the average particle size is 74 um, and the particle size distribution is D±5 um.

[0049] The spinning liquid is added to the feeding port of the twin screw, where: the twin screw diameter is 50 mm, the aspect ratio is 60, the screw speed is set to 550 RPM, the twin screw feeding section temperature is set to 130, 150, 160°C, the compression section temperature is set to 170, 175, 180, 180, 180°C, and the homogenization section temperature is set to 180, 180, 180°C.

[0050] The spinning solution is dissolved by a twin-screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle for drawing, and a coagulation bath to obtain primary frozen gel filaments; wherein, the distance between the spinneret and the coagulation bath is 5.0 cm, the coagulation bath is a 0.1% NP-9 aqueous solution, the coagulation bath temperature is 5°C, and the number of spinneret holes is 200.

[0051] After the primary jelly fibers are extracted, they are blown with high-pressure hot air and then quickly passed into a constant temperature water bath with ultrasonic function, where the high-pressure hot air temperature is 40°C, the water bath temperature is 75°C, and the ultrasonic power is 4500W. The effective stretching length of the fiber in the constant temperature water bath is 4 meters, and the fiber stretching multiple in the constant temperature water bath is 2.5 times.

[0052] The fibers derived from the constant temperature water bath were blown with compressed air to remove water from the fiber surface, and then were drawn through 4 stages of hot box to obtain ultra-high molecular weight polyethylene fibers, wherein the temperatures of the 4 stages of hot boxes were 110, 120, 140, and 145°C, respectively, and the total hot box drawing multiple was 32 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers were tested. The fiber breaking strength was 42.6 cN / dtex, the initial modulus was 1830 cN / dtex, the fiber adhesion rate was 2.0%, the fiber molecular weight was 3760000 g / mol, and the molecular weight distribution was 2.8.

[0053] Example 2

[0054] 10kg of ultra-high molecular weight polyethylene powder with a molecular weight of 8900000g / mol, 190kg of kerosene and 100g of tris[2,4-di-tert-butylphenyl]phosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 5%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the ultra-high molecular weight polyethylene powder has a molecular weight distribution of 1.9, a bulk density of 0.45g / cm3, an average particle size of 78um and a particle size distribution of D±5um.

[0055] The spinning liquid is added to the feeding port of the twin screw through a pipe, wherein: the diameter of the twin screw is 70 mm, the aspect ratio is 56, the screw speed is set to 600 RPM, the temperature of the twin screw feeding section is set to 100, 130, 160°C, the temperature of the compression section is set to 160, 180, 180, 180, 180°C, and the temperature of the homogenization section is set to 180, 180, 170°C.

[0056] The spinning solution is dissolved by a twin screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle drafting, and a coagulation bath to obtain primary gel filaments. The distance between the spinneret and the coagulation bath is 10 cm, the coagulation bath is a 0.15% NP-10 aqueous solution, the coagulation bath temperature is 15°C, and the number of spinneret holes is 240.

[0057] After the primary jelly fibers are extracted, they are blown with high-pressure hot air and then quickly passed into a constant temperature water bath with ultrasonic function, where the high-pressure hot air temperature is 100°C, the water bath temperature is 85°C, and the ultrasonic power is 4500W. The effective stretching length of the fiber in the constant temperature water bath is 4 meters, and the fiber stretching multiple in the constant temperature water bath is 3.4 times.

[0058] The fibers derived from the constant temperature water bath were blown with compressed air to remove water from the fiber surface, and then were drawn through 4 stages of hot box to obtain ultra-high molecular weight polyethylene fibers, wherein the temperatures of the 4 stages of hot boxes were 120, 130, 140, and 148°C, respectively, and the total hot box drawing multiple was 26 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers were tested. The fiber breaking strength was 44.3 cN / dtex, the initial modulus was 1890 cN / dtex, the fiber adhesion rate was 1.25%, the fiber molecular weight was 4150000 g / mol, and the molecular weight distribution was 2.5.

[0059] Embodiment 3 (best embodiment)

[0060] 16 kg of ultra-high molecular weight polyethylene powder with a molecular weight of 8500000 g / mol, 184 kg of liquid paraffin, 40 g of tris[2,4-di-tert-butylphenyl]phosphite and 40 g of distearyl pentaerythritol diphosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 8%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the ultra-high molecular weight polyethylene powder has a molecular weight distribution of 1.7, a bulk density of 0.46 g / cm3, an average particle size of 75 um and a particle size distribution of D±5 um.

[0061] The spinning liquid is added to the feeding port of the twin screw through a pipe, wherein: the twin screw diameter is 65 mm, the aspect ratio is 64, the screw speed is set to 750 RPM, the twin screw feeding section temperature is set to 110, 130, 150°C, the compression section temperature is set to 160, 165, 170, 175, 175°C, and the homogenization section temperature is set to 175, 175, 170°C.

[0062] The spinning solution is dissolved by a twin screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle drafting, and a coagulation bath to obtain primary gel filaments. The distance between the spinneret and the coagulation bath is 3.0 cm, the coagulation bath is a 0.05% NP-10 aqueous solution, the coagulation bath temperature is 10°C, and the number of spinneret holes is 320.

[0063] After the primary jelly fibers are extracted, they are blown with high-pressure hot air and then quickly passed into a constant temperature water bath with ultrasonic function. The high-pressure hot air temperature is 65°C, the water bath temperature is 90°C, and the ultrasonic power is 4500W. The effective stretching length of the fiber in the constant temperature water bath is 4 meters, and the fiber stretching multiple in the constant temperature water bath is 3.8 times.

[0064] The fibers derived from the constant temperature water bath were blown with compressed air to remove water from the fiber surface, and then were drawn through 4 stages of hot box to obtain ultra-high molecular weight polyethylene fibers, wherein the temperatures of the 4 stages of hot boxes were 110, 130, 145, and 148°C, respectively, and the total hot box drawing multiple was 28 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers were tested. The fiber breaking strength was 45.2 cN / dtex, the initial modulus was 1920 cN / dtex, the fiber adhesion rate was 0.94%, the fiber molecular weight was 4210000 g / mol, and the molecular weight distribution was 2.2.

[0065] Example 4

[0066] 12kg of ultra-high molecular weight polyethylene powder with a molecular weight of 6200000g / mol, 188kg of decalin and 30g of distearyl pentaerythritol diphosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 6%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the ultra-high molecular weight polyethylene powder has a molecular weight distribution of 2.5, a bulk density of 0.41g / cm3, an average particle size of 69um and a particle size distribution of D±5um.

[0067] The spinning liquid is added to the feeding port of the twin screw through a pipe, wherein: the diameter of the twin screw is 90 mm, the aspect ratio is 64, the screw speed is set to 750 RPM, the temperature of the twin screw feeding section is set to 110, 130, 150°C, the temperature of the compression section is set to 160, 165, 170, 175, 175°C, and the temperature of the homogenizing section is set to 175, 175, 170°C.

[0068] The spinning solution is dissolved by a twin screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle drafting, and a coagulation bath to obtain primary jelly filaments. The distance between the spinneret and the coagulation bath is 2.0 cm, the coagulation bath is a 0.05% TX-10 aqueous solution, the coagulation bath temperature is 3°C, and the number of spinneret holes is 320.

[0069] After the primary jelly fibers are extracted, they are blown with high-pressure hot air and then quickly passed into a constant temperature water bath with ultrasonic function, where the high-pressure hot air temperature is 70°C, the water bath temperature is 95°C, and the ultrasonic power is 4500W. The effective stretching length of the fiber in the constant temperature water bath is 4 meters, and the fiber stretching multiple in the constant temperature water bath is 4.5 times.

[0070] The fibers derived from the constant temperature water bath were blown with compressed air to remove water from the fiber surface, and then were drawn through 4 stages of hot box to obtain ultra-high molecular weight polyethylene fibers, wherein the temperatures of the 4 stages of hot boxes were 110, 130, 145, and 148°C, respectively, and the total hot box drawing multiple was 24 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers were tested. The fiber breaking strength was 42.4 cN / dtex, the initial modulus was 1820 cN / dtex, the fiber adhesion rate was 2.5%, the fiber molecular weight was 3820000 g / mol, and the molecular weight distribution was 3.2.

[0071] Example 5

[0072] 24 kg of ultra-high molecular weight polyethylene powder with a molecular weight of 5500000 g / mol, 176 kg of liquid paraffin, 60 g of tris[2,4-di-tert-butylphenyl]phosphite and 60 g of distearyl pentaerythritol diphosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 12%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the ultra-high molecular weight polyethylene powder has a molecular weight distribution of 2.4, a bulk density of 0.45 g / cm3, an average particle size of 65 um and a particle size distribution of D±5 um.

[0073] The spinning solution is added to the feeding port of the twin screw through a pipe, wherein: the twin screw diameter is 115 mm, the aspect ratio is 60, the screw speed is set to 680 RPM, the twin screw feeding section temperature is set to 110, 130, 150°C, the compression section temperature is set to 160, 165, 170, 180, 180°C, and the homogenization section temperature is set to 180, 175, 170°C.

[0074] The spinning solution is dissolved by a twin screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle drafting, and a coagulation bath to obtain primary jelly filaments. The distance between the spinneret and the coagulation bath is 15 cm, the coagulation bath is a 0.03% NP-9 aqueous solution, the coagulation bath temperature is 10°C, and the number of spinneret holes is 320.

[0075] After the primary jelly fibers are extracted, they are blown with high-pressure hot air and then quickly passed into a constant temperature water bath with ultrasonic function, where the high-pressure hot air temperature is 50°C, the water bath temperature is 55°C, and the ultrasonic power is 4500W. The effective stretching length of the fiber in the constant temperature water bath is 4 meters, and the fiber stretching multiple in the constant temperature water bath is 1.5 times.

[0076] The fibers derived from the constant temperature water bath were blown away with compressed air to remove water from the fiber surface, and then were drawn through 4 stages of hot box drawing to obtain ultra-high molecular weight polyethylene fibers, wherein the temperatures of the 4 stages of hot boxes were 110, 130, 140, and 147°C, respectively, and the total hot box drawing multiple was 33 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers were tested. The fiber breaking strength was 42.2 cN / dtex, the initial modulus was 1810 cN / dtex, the fiber adhesion rate was 2.19%, the fiber molecular weight was 3530000 g / mol, and the molecular weight distribution was 2.9.

[0077] Comparative Example 1 (the raw materials have been optimized, and the extracted fibers are dried in a drying oven)

[0078] 16 kg of ultra-high molecular weight polyethylene powder with a molecular weight of 8500000 g / mol, 184 kg of liquid paraffin, 40 g of tris[2,4-di-tert-butylphenyl]phosphite and 40 g of distearyl pentaerythritol diphosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 8%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the ultra-high molecular weight polyethylene powder has a molecular weight distribution of 1.7, a bulk density of 0.46 g / cm3, an average particle size of 75 um and a particle size distribution of D±5 um.

[0079] The spinning liquid is added to the feeding port of the twin screw through a pipe, wherein: the twin screw diameter is 65 mm, the aspect ratio is 64, the screw speed is set to 750 RPM, the twin screw feeding section temperature is set to 110, 130, 150°C, the compression section temperature is set to 160, 165, 170, 175, 175°C, and the homogenization section temperature is set to 175, 175, 170°C.

[0080] The spinning solution is dissolved by a twin screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle drafting, and a coagulation bath to obtain primary gel filaments. The distance between the spinneret and the coagulation bath is 3.0 cm, the coagulation bath is a 0.05% NP-10 aqueous solution, the coagulation bath temperature is 10°C, and the number of spinneret holes is 320.

[0081] After extraction, the primary frozen gel fibers are dried in a drying oven and then drawn in a 4-stage hot box to obtain ultra-high molecular weight polyethylene fibers. The temperatures of the 4-stage hot boxes are 110, 130, 145, and 148°C, respectively, and the total hot box drawing multiple is 28 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers are tested. The fiber breaking strength is 37.8 cN / dtex, the initial modulus is 1680 cN / dtex, the fiber adhesion rate is 12.19%, the fiber molecular weight is 4160000 g / mol, and the molecular weight distribution is 2.3.

[0082] Comparative Example 2 (drying using a constant temperature water bath with a lower water temperature in the water bath)

[0083] 16 kg of ultra-high molecular weight polyethylene powder with a molecular weight of 8500000 g / mol, 184 kg of liquid paraffin, 40 g of tris[2,4-di-tert-butylphenyl]phosphite and 40 g of distearyl pentaerythritol diphosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 8%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the ultra-high molecular weight polyethylene powder has a molecular weight distribution of 1.7, a bulk density of 0.46 g / cm3, an average particle size of 75 um and a particle size distribution of D±5 um.

[0084] The spinning liquid is added to the feeding port of the twin screw through a pipe, wherein: the twin screw diameter is 65 mm, the aspect ratio is 64, the screw speed is set to 750 RPM, the twin screw feeding section temperature is set to 110, 130, 150°C, the compression section temperature is set to 160, 165, 170, 175, 175°C, and the homogenization section temperature is set to 175, 175, 170°C.

[0085] The spinning solution is dissolved by a twin screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle drafting, and a coagulation bath to obtain primary gel filaments. The distance between the spinneret and the coagulation bath is 3.0 cm, the coagulation bath is a 0.05% NP-10 aqueous solution, the coagulation bath temperature is 10°C, and the number of spinneret holes is 320.

[0086] After the primary jelly fibers are extracted, they are blown with high-pressure hot air and then quickly passed into a constant temperature water bath with ultrasonic function, where the high-pressure hot air temperature is 65°C, the water bath temperature is 35°C, and the ultrasonic power is 4500W. The effective stretching length of the fiber in the constant temperature water bath is 4 meters, and the fiber stretching multiple in the constant temperature water bath is 3.8 times.

[0087] The fibers derived from the constant temperature water bath were blown with compressed air to remove water from the fiber surface, and then were drawn through 4 stages of hot box drawing to obtain ultra-high molecular weight polyethylene fibers, wherein the temperatures of the 4 stages of hot boxes were 110, 130, 145, and 148°C, respectively, and the total hot box drawing multiple was 28 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers were tested. The fiber breaking strength was 38.5 cN / dtex, the initial modulus was 1720 cN / dtex, the fiber adhesion rate was 6.56%, the fiber molecular weight was 4200000 g / mol, and the molecular weight distribution was 2.2.

[0088] Comparative Example 3 (Drying in a constant temperature water bath without ultrasound in the water bath)

[0089] 16 kg of ultra-high molecular weight polyethylene powder with a molecular weight of 8500000 g / mol, 184 kg of liquid paraffin, 40 g of tris[2,4-di-tert-butylphenyl]phosphite and 40 g of distearyl pentaerythritol diphosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 8%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the ultra-high molecular weight polyethylene powder has a molecular weight distribution of 1.7, a bulk density of 0.46 g / cm3, an average particle size of 75 um and a particle size distribution of D±5 um.

[0090] The spinning liquid is added to the feeding port of the twin screw through a pipe, wherein: the twin screw diameter is 65 mm, the aspect ratio is 64, the screw speed is set to 750 RPM, the twin screw feeding section temperature is set to 110, 130, 150°C, the compression section temperature is set to 160, 165, 170, 175, 175°C, and the homogenization section temperature is set to 175, 175, 170°C.

[0091] The spinning solution is dissolved by a twin screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle drafting, and a coagulation bath to obtain primary gel filaments. The distance between the spinneret and the coagulation bath is 3.0 cm, the coagulation bath is a 0.05% NP-10 aqueous solution, the coagulation bath temperature is 10°C, and the number of spinneret holes is 320.

[0092] After the primary jelly fibers are extracted, they are blown with high-pressure hot air and then quickly passed into a constant temperature water bath with ultrasonic function. The high-pressure hot air temperature is 65°C, the water bath temperature is 90°C, the effective stretching length of the fibers in the constant temperature water bath is 4 meters, and the stretching multiple of the fibers in the constant temperature water bath is 3.8 times.

[0093] The fibers derived from the constant temperature water bath were blown with compressed air to remove water from the fiber surface, and then were drawn through 4 stages of hot box to obtain ultra-high molecular weight polyethylene fibers, wherein the temperatures of the 4 stages of hot boxes were 110, 130, 145, and 148°C, respectively, and the total hot box drawing multiple was 28 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers were tested. The fiber breaking strength was 39.3 cN / dtex, the initial modulus was 1750 cN / dtex, the fiber adhesion rate was 5.31%, the fiber molecular weight was 4210000 g / mol, and the molecular weight distribution was 2.2.

[0094] Comparative Example 4 (Drying with a constant temperature water bath, without drawing the fiber in the constant temperature water bath)

[0095] 16 kg of ultra-high molecular weight polyethylene powder with a molecular weight of 8500000 g / mol, 184 kg of liquid paraffin, 40 g of tris[2,4-di-tert-butylphenyl]phosphite and 40 g of distearyl pentaerythritol diphosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 8%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the ultra-high molecular weight polyethylene powder has a molecular weight distribution of 1.7, a bulk density of 0.46 g / cm3, an average particle size of 75 um and a particle size distribution of D±5 um.

[0096] The spinning liquid is added to the feeding port of the twin screw through a pipe, wherein: the twin screw diameter is 65 mm, the aspect ratio is 64, the screw speed is set to 750 RPM, the twin screw feeding section temperature is set to 110, 130, 150°C, the compression section temperature is set to 160, 165, 170, 175, 175°C, and the homogenization section temperature is set to 175, 175, 170°C.

[0097] The spinning solution is dissolved by a twin screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle drafting, and a coagulation bath to obtain primary gel filaments. The distance between the spinneret and the coagulation bath is 3.0 cm, the coagulation bath is a 0.05% NP-10 aqueous solution, the coagulation bath temperature is 10°C, and the number of spinneret holes is 320.

[0098] After the primary jelly fibers are extracted, they are blown with high-pressure hot air and then quickly passed into a constant-temperature water bath with ultrasonic function, where the high-pressure hot air temperature is 65°C, the water bath temperature is 90°C, the ultrasonic power is 4500W, the effective stretching length of the fiber in the constant-temperature water bath is 4 meters, and the fiber stretching multiple in the constant-temperature water bath is 1.0 times.

[0099] The fibers derived from the constant temperature water bath were blown with compressed air to remove water from the fiber surface, and then were drawn through 4 stages of hot box to obtain ultra-high molecular weight polyethylene fibers, wherein the temperatures of the 4 stages of hot boxes were 110, 130, 145, and 148°C, respectively, and the total hot box drawing multiple was 28 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers were tested. The fiber breaking strength was 40.7 cN / dtex, the initial modulus was 1770 cN / dtex, the fiber adhesion rate was 5.63%, the fiber molecular weight was 4210000 g / mol, and the molecular weight distribution was 2.2.

[0100] Comparative Example 5 (Drying with a constant temperature water bath, the fiber drafting multiple in the constant temperature water bath is too high)

[0101] 16 kg of ultra-high molecular weight polyethylene powder with a molecular weight of 8500000 g / mol, 184 kg of liquid paraffin, 40 g of tris[2,4-di-tert-butylphenyl]phosphite and 40 g of distearyl pentaerythritol diphosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 8%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the ultra-high molecular weight polyethylene powder has a molecular weight distribution of 1.7, a bulk density of 0.46 g / cm3, an average particle size of 75 um and a particle size distribution of D±5 um.

[0102] The spinning liquid is added to the feeding port of the twin screw through a pipe, wherein: the twin screw diameter is 65 mm, the aspect ratio is 64, the screw speed is set to 750 RPM, the twin screw feeding section temperature is set to 110, 130, 150°C, the compression section temperature is set to 160, 165, 170, 175, 175°C, and the homogenization section temperature is set to 175, 175, 170°C.

[0103] The spinning solution is dissolved by a twin screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle drafting, and a coagulation bath to obtain primary gel filaments. The distance between the spinneret and the coagulation bath is 3.0 cm, the coagulation bath is a 0.05% NP-10 aqueous solution, the coagulation bath temperature is 10°C, and the number of spinneret holes is 320.

[0104] After the primary jelly fibers are extracted, they are blown with high-pressure hot air and then quickly passed into a constant temperature water bath with ultrasonic function. The high-pressure hot air temperature is 65°C, the water bath temperature is 90°C, and the ultrasonic power is 4500W. The effective stretching length of the fiber in the constant temperature water bath is 4 meters, and the fiber stretching multiple in the constant temperature water bath is 7 times.

[0105] The fibers derived from the constant temperature water bath were blown away with compressed air to remove water from the fiber surface, and then were drawn through 4 stages of hot box drawing to obtain ultra-high molecular weight polyethylene fibers, wherein the temperatures of the 4 stages of hot boxes were 110, 130, 145, and 148°C, respectively, and the total hot box drawing multiple was 28 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers were tested. The fiber breaking strength was 38.9 cN / dtex, the initial modulus was 1750 cN / dtex, the fiber adhesion rate was 3.25%, the fiber molecular weight was 3460000 g / mol, and the molecular weight distribution was 3.6.

[0106] Comparative Example 6 (Raw materials not preferred)

[0107] 16 kg of ultra-high molecular weight polyethylene powder with a molecular weight of 4600000 g / mol, 184 kg of liquid paraffin, 40 g of tris[2,4-di-tert-butylphenyl]phosphite and 40 g of distearyl pentaerythritol diphosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 8%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the ultra-high molecular weight polyethylene powder has a molecular weight distribution of 3.8, a bulk density of 0.49 g / cm3, an average particle size of 72 um and a particle size distribution of D±5 um.

[0108] The spinning liquid is added to the feeding port of the twin screw through a pipe, wherein: the twin screw diameter is 65 mm, the aspect ratio is 64, the screw speed is set to 750 RPM, the twin screw feeding section temperature is set to 110, 130, 150°C, the compression section temperature is set to 160, 165, 170, 175, 175°C, and the homogenization section temperature is set to 175, 175, 170°C.

[0109] The spinning solution is dissolved by a twin screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle drafting, and a coagulation bath to obtain primary gel filaments. The distance between the spinneret and the coagulation bath is 3.0 cm, the coagulation bath is a 0.05% NP-10 aqueous solution, the coagulation bath temperature is 10°C, and the number of spinneret holes is 320.

[0110] After the primary jelly fibers are extracted, they are blown with high-pressure hot air and then quickly passed into a constant temperature water bath with ultrasonic function, where the high-pressure hot air temperature is 65°C, the water bath temperature is 90°C, and the ultrasonic power is 4500W. The effective stretching length of the fiber in the constant temperature water bath is 4 meters, and the fiber stretching multiple in the constant temperature water bath is 3.8 times.

[0111] The fibers derived from the constant temperature water bath were blown with compressed air to remove water from the fiber surface, and then were drawn through 4 stages of hot box to obtain ultra-high molecular weight polyethylene fibers, wherein the temperatures of the 4 stages of hot boxes were 110, 130, 145, and 148°C, respectively, and the total hot box drawing multiple was 28 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers were tested. The fiber breaking strength was 38.5 cN / dtex, the initial modulus was 1710 cN / dtex, the fiber adhesion rate was 16.9%, the fiber molecular weight was 2840000 g / mol, and the molecular weight distribution was 4.3.

[0112] Comparative Example 7 (Raw materials not preferred)

[0113] 16 kg of ultra-high molecular weight polyethylene powder with a molecular weight of 9600000 g / mol, 184 kg of liquid paraffin, 40 g of tris[2,4-di-tert-butylphenyl]phosphite and 40 g of distearyl pentaerythritol diphosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 8%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the ultra-high molecular weight polyethylene powder has a molecular weight distribution of 3.5, a bulk density of 0.44 g / cm3, an average particle size of 78 um and a particle size distribution of D±5 um.

[0114] The spinning liquid is added to the feeding port of the twin screw through a pipe, wherein: the twin screw diameter is 65 mm, the aspect ratio is 64, the screw speed is set to 750 RPM, the twin screw feeding section temperature is set to 110, 130, 150°C, the compression section temperature is set to 160, 165, 170, 175, 175°C, and the homogenization section temperature is set to 175, 175, 170°C.

[0115] The spinning solution is dissolved by a twin screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle drafting, and a coagulation bath to obtain primary gel filaments. The distance between the spinneret and the coagulation bath is 3.0 cm, the coagulation bath is a 0.05% NP-10 aqueous solution, the coagulation bath temperature is 10°C, and the number of spinneret holes is 320.

[0116] After the primary jelly fibers are extracted, they are blown with high-pressure hot air and then quickly passed into a constant temperature water bath with ultrasonic function, where the high-pressure hot air temperature is 65°C, the water bath temperature is 90°C, and the ultrasonic power is 4500W. The effective stretching length of the fiber in the constant temperature water bath is 4 meters, and the fiber stretching multiple in the constant temperature water bath is 3.8 times.

[0117] The fibers derived from the constant temperature water bath were blown with compressed air to remove water from the fiber surface, and then were drawn through 4 stages of hot box to obtain ultra-high molecular weight polyethylene fibers, wherein the temperatures of the 4 stages of hot boxes were 110, 130, 145, and 148°C, respectively, and the total hot box drawing multiple was 28 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers were tested. The fiber breaking strength was 41.2 cN / dtex, the initial modulus was 1780 cN / dtex, the fiber adhesion rate was 7.8%, the fiber molecular weight was 4140000 g / mol, and the molecular weight distribution was 3.9.

[0118] Comparative Example 8 (Spinning solution concentration is too high)

[0119] 30 kg of ultra-high molecular weight polyethylene powder with a molecular weight of 8500000 g / mol, 170 kg of liquid paraffin, 75 g of tris[2,4-di-tert-butylphenyl]phosphite and 75 g of distearyl pentaerythritol diphosphite are added into a high-speed emulsifier, mixed evenly by the high-speed emulsifier and then transferred to a feeding kettle to obtain a spinning solution with an ultra-high molecular weight polyethylene concentration of 15%; the swelling kettle is evacuated and nitrogen is passed through for 3 times to replace the air in the swelling kettle and the solution, wherein the ultra-high molecular weight polyethylene powder has a molecular weight distribution of 1.7, a bulk density of 0.46 g / cm3, an average particle size of 75 um and a particle size distribution of D±5 um.

[0120] The spinning liquid is added to the feeding port of the twin screw through a pipe, wherein: the twin screw diameter is 65 mm, the aspect ratio is 64, the screw speed is set to 750 RPM, the twin screw feeding section temperature is set to 110, 130, 150°C, the compression section temperature is set to 160, 165, 170, 175, 175°C, and the homogenization section temperature is set to 175, 175, 170°C.

[0121] The spinning solution is dissolved by a twin screw extruder, quantitatively extruded by a metering pump, and then passed through a spinneret, a nozzle drafting, and a coagulation bath to obtain primary gel filaments. The distance between the spinneret and the coagulation bath is 3.0 cm, the coagulation bath is a 0.05% NP-10 aqueous solution, the coagulation bath temperature is 10°C, and the number of spinneret holes is 320.

[0122] After the primary jelly fibers are extracted, they are blown with high-pressure hot air and then quickly passed into a constant temperature water bath with ultrasonic function, where the high-pressure hot air temperature is 65°C, the water bath temperature is 90°C, and the ultrasonic power is 4500W. The effective stretching length of the fiber in the constant temperature water bath is 4 meters, and the fiber stretching multiple in the constant temperature water bath is 3.8 times.

[0123] The fibers derived from the constant temperature water bath were blown with compressed air to remove water from the fiber surface, and then were drawn through 4 stages of hot box to obtain ultra-high molecular weight polyethylene fibers, wherein the temperatures of the 4 stages of hot boxes were 110, 130, 145, and 148°C, respectively, and the total hot box drawing multiple was 28 times. The mechanical properties, adhesion rate, molecular weight and its distribution of the fibers were tested. The fiber breaking strength was 36.7 cN / dtex, the initial modulus was 1630 cN / dtex, the fiber adhesion rate was 1.88%, the fiber molecular weight was 3910000 g / mol, and the molecular weight distribution was 2.8.

[0124] The inventors discovered during the production process that the adhesion of ultra-high molecular weight polyethylene fibers mainly occurs during the drying process after the extraction of the primary fibers. The ultra-high molecular weight polyethylene fibers are in a swollen state in the extraction tank. During the dissolution process, the low molecular weight molecular chains obtained due to the breakage of the molecular chains diffuse to the fiber surface as the extractant evaporates and migrate to the fiber surface. When the low molecular weight ultra-high molecular weight polyethylene molecular chains in the two fibers contact on the fiber surface, entanglement occurs, resulting in the adhesion of the two fibers.

[0125] The present invention proposes for the first time a method for reducing the adhesion of ultra-high molecular weight polyethylene fibers, by selecting ultra-high molecular weight polyethylene raw materials, and setting a constant temperature water bath with a high-power ultrasonic function after the jelly silk extraction, and controlling the fiber tension in the constant temperature water bath. The ultrasonic stripping effect and the application of appropriate tension separate adjacent fibers, and then a hot water bath is used to quickly evaporate the extractant on the fiber surface, so that when the small molecule ultra-high molecular weight polyethylene molecular chains have not yet migrated to the fiber surface, the extractant on the fiber surface has been completely evaporated, thereby preventing the migration of small molecule chains to the fiber surface and greatly reducing the problem of adhesion between fibers.

[0126] Surprisingly, when the fiber paralleling ratio is greatly reduced, the mechanical properties of the fiber are correspondingly improved due to the reduction of stress concentration points.

[0127] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.

Claims

1. A method for reducing adhesion of ultra-high molecular weight polyethylene fibers, Features: include, After the primary jelly silk is extracted through an extraction tank, a fiber bundle containing a large amount of extractant inside and on the surface is obtained; After the extracted fiber bundle is purged with high-pressure hot air, it is passed into a water bath thermostatic bath with ultrasonic function, the high-pressure hot air temperature is 40-100°C, the ultrasonic power is ≥4000W, the water bath temperature is 50-99°C, the effective distance of the fiber bundle in the water bath is ≥4 meters, and the draft ratio of the fiber bundle in the water bath is 1.2-5.0; The fiber tow passes through a water bath thermostatic tank to quickly remove the extractant and is heat-stretched, then blown with compressed air to remove surface moisture, and then passed through a heat box for super-high heat stretching to obtain ultra-high molecular weight polyethylene fibers; Among them, the super-multiple hot stretching is carried out through a hot box, wherein a 4-stage hot box stretching is adopted, the effective heating length of each hot box is 4 meters, the internal temperature of the hot box is 100-150°C, and the total hot box stretching multiple is 15-40 times.

2. The method according to claim 1, Features: The preparation method of the primary jelly silk comprises: Ultra-high molecular weight polyethylene powder, spinning solvent and antioxidant are added to a high-speed mixer and mixed evenly, and then added to a feeding kettle, and then the feeding kettle is evacuated and nitrogen is passed through for three times to replace the air in the feeding kettle and the solvent to obtain a spinning solution; The obtained spinning solution is added to the feeding port of the twin-screw extruder, dissolved by the twin-screw extruder, quantitatively extruded by the metering pump, and then passed through the spinneret, nozzle drawing, coagulation bath, and collected to obtain the primary jelly filaments.

3. The method according to claim 2, Features: The molecular weight of the ultra-high molecular weight polyethylene powder is 5000000-9000000 g / mol, and the molecular weight distribution is 1.5-2.5; the bulk density of the ultra-high molecular weight polyethylene powder is 0.30-0.50 g / cm 3 The average particle size is D≤80um and the particle size distribution is D±5um; the ultra-high molecular weight polyethylene powder accounts for 5 to 12wt% of the total mass of the mixed spinning solution.

4. The method according to claim 2, Features: The coagulation bath is a mixture of water and nonionic surfactant, wherein the nonionic surfactant is one or a mixture of NP-9, NP-10, and TX-10, and the nonionic surfactant accounts for 0.01 to 0.15 wt % of the total mass of the coagulation bath. The temperature of the coagulation bath is 0 to 15° C.

5. The method according to claim 2, Features: The spinning solvent is one or more hydrocarbons, including one or more of decalin, tetralin, kerosene and liquid paraffin.

6. The method according to claim 2, Features: The antioxidant is one or a mixture of phenolic antioxidants and phosphite antioxidants, including one or a mixture of tris[2,4-di-tert-butylphenyl]phosphite, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol, β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 2,6-di-tert-butyl-4-methylphenol, distearyl pentaerythritol diphosphite; the antioxidant is added in an amount of 0.1-1.0wt% of the mass of the ultra-high molecular weight polyethylene powder.

7. The method according to claim 2, Features: The method for preparing primary jelly silk comprises: Screw diameter 36-150mm, aspect ratio 45-65; Screw speed: 400~1200RPM; The temperature of the screw feeding section is 90-160°C, the temperature of the screw compression section is 160-180°C, and the temperature of the screw homogenization section is 170-180°C; The number of holes of the spinneret is 2 to 2000, and the height from the spinneret to the surface of the coagulation bath is 1 to 15 cm.

8. The method according to claim 1, Features: The extractant is one or more combinations of xylene, dichloromethane, carbon tetrachloride, dichloroethane, n-hexane, gasoline, and hydrocarbon cleaning agent, and the extraction temperature is 20-50°C.

9. The method according to any one of claims 1 to 8, Features: The ultra-high molecular weight polyethylene fiber has a bonding rate of ≤3%, a fiber breaking strength of ≥42 cN / dtex, an initial modulus of ≥1800 cN / dtex, a molecular weight of ≥3500000 g / mol, and a molecular weight distribution of 2.0-3.5.

Citation Information

Patent Citations

  • Method for reducing doubling rate of ultra-high molecular weight polyethylene fiber in manufacturing process, fiber and fabric

    CN114293276A

  • Preparation method of polyethylene fibers with wide width, high strength and high modulus

    CN110079872A

  • Preparation method of civil high-performance polyethylene fiber

    CN110820058A