Composite lithium supplement material and preparation method and application thereof
By doping non-carbon heteroatoms into carbon materials and growing metal compounds, forming a highly conductive catalyst and combining lithium-rich materials, the problem of insufficient activity and conductivity of existing lithium-enhancing materials is solved, and the circulation of batteries is significantly improved Performance and energy density.
Patent Information
- Application Number
- CN202410242266.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-04
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-03-04
AI Technical Summary
The existing lithium supplementary material catalysts have low catalytic activity and poor conductivity, resulting in the inability to effectively release lithium ions under low voltage conditions and poor kinetic performance.
Using a composite catalyst of carbon material and metal compounds, a high conductivity and high catalytic activity catalyst is formed by doping non-carbon heteroatoms into the carbon material and growing metal compounds on it, combining lithium-rich materials to form composite lithium supplementation Material.
The conductivity and catalytic activity of the catalyst are improved, the decomposition voltage of lithium-rich materials is reduced, the catalytic efficiency is enhanced, and the circulation performance and energy density of the battery are improved.
Smart Images

Figure CN118142560B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of secondary batteries, and in particular to a composite lithium supplement material and a preparation method and application thereof. Background Art
[0002] During the first charge and discharge process of the battery, the electrolyte will undergo a reduction decomposition reaction on the surface of the negative electrode and form a layer of solid electrolyte interface film (SEI film). The formation of the SEI film will consume a large amount of active lithium, resulting in a decrease in the actual energy density of the battery compared to the theoretical calculated value. During the battery's cyclic charge and discharge process, the cracking and crushing of the positive electrode active material particles, the thickening and repair of the SEI film will continuously consume active lithium, causing a continuous decline in the battery's cycle performance. In order to further improve the battery's energy density and cycle performance, adding lithium supplement materials to the positive electrode plate can effectively alleviate the problems of low battery energy density, low first-cycle efficiency, and poor cycle life.
[0003] However, the current lithium-supplementing materials have problems such as high decomposition voltage and poor conductivity, which make it impossible for lithium-supplementing materials to fully release lithium ions under low voltage conditions, and the transmission path of electrons and ions in lithium-supplementing materials is long, and the kinetic performance is poor. Therefore, catalysts are added to the existing lithium-supplementing materials to reduce the delithiation potential of lithium-rich materials in lithium-supplementing materials. However, most catalysts have limited catalytic activity themselves, making it difficult to achieve the desired effect, and the catalysts have limited improvement in the conductivity of lithium-rich materials, so how to provide a catalyst with high catalytic activity and conductivity has become the key. Summary of the invention
[0004] The purpose of the present invention is to provide a composite lithium supplement material and a preparation method and application thereof, so as to solve the problem of low catalytic activity or poor conductivity of the catalyst.
[0005] To achieve the purpose of the present invention, the present invention provides the following technical solutions:
[0006] In a first aspect, the present invention provides a catalyst comprising a carbon material and a metal compound; wherein the carbon material is doped with heteroatoms of non-carbon elements; and the metal compound grows on the carbon material.
[0007] The catalyst provided by the present application includes a carbon material and a metal compound, wherein the carbon material is doped with heteroatoms, and the metal compound grows on the carbon material. The catalyst provided by the present application has the following advantages: 1) The catalyst has both electrical conductivity and catalytic ability. The existing catalytic materials only have catalytic compounds, so the catalytic materials only provide catalytic ability. The present application combines the carbon material and the metal compound, and utilizes the high electrical conductivity of the carbon material itself, so that the catalyst has electrical conductivity. After the catalyst is combined with the lithium-rich material, there is no need to add conductive material; 2) The carbon material in the catalyst has higher electrical conductivity and catalytic activity. Through heteroatom doping, because the doping of heteroatoms can change the electronic structure and chemical properties of the carbon material, its electrical conductivity, catalytic activity, etc. are improved, compared with the pure carbon material in the prior art. In other words, the doped carbon material can play a synergistic role with the metal compound to improve the comprehensive performance of the catalyst; 3) The production process of the metal compound directly growing on the carbon material is simple, and the bonding strength between the metal compound and the carbon material is high. Compared with the simply mixed composite catalyst in the prior art, the metal compound provided by the present invention is not easy to fall off from the carbon material, so the catalyst has high stability when used; 4) By loading the metal compound on the carbon material by direct growth, a larger metal compound loading amount can be obtained on the carbon material, because compared with the physical mixing method, the grown metal compound is more likely to form a densely packed structure, and the metal compound is more densely attached, thereby increasing the loading amount of the metal compound on the carbon material, so the metal compound content in the catalyst provided by the present invention is higher and the catalytic efficiency is higher.
[0008] In one embodiment, the loading amount of the metal compound per unit area of the carbon material is greater than or equal to 10 wt %.
[0009] In a second aspect, the present invention provides a composite lithium supplement material, comprising a lithium-rich material and the catalyst provided in the first aspect, wherein the catalyst is combined with the lithium-rich material.
[0010] The present invention combines the catalyst provided by the above-mentioned embodiment with a lithium-rich material to obtain a composite lithium-supplementing material, which has the following effects: 1) The lithium-rich material can have a high loading of catalyst. Based on the structure of the catalyst, since the content of metal compounds in the catalyst is higher, in the lithium-supplementing material of the same volume, the composite lithium-supplementing material provided by the present invention has more catalysts, and the catalytic effect of the catalyst on the lithium-rich material is enhanced, so that the decomposition voltage of the lithium-rich material decreases more significantly; 2) The lithium-rich material and the catalyst are more closely combined. Since the carbon material in the catalyst can provide a larger specific surface area, the carbon material will have more active sites. The lithium-rich material, the carbon material and the metal compound are firmly combined together by intermolecular forces. The metal compound is not easy to fall off the carbon material, and the catalyst as a whole is not easy to fall off the lithium-rich material. Therefore, in the process of the catalyst catalyzing the lithium-rich material, the catalytic effect of the catalyst is enhanced, and the decomposition voltage of the lithium-rich material can be further reduced.
[0011] In one embodiment, the non-carbon element heteroatom includes a non-metallic heteroatom, and the non-metallic heteroatom is connected to the carbon atom of the carbon material through a chemical bond.
[0012] In one embodiment, the non-carbon element heteroatom further includes a metal heteroatom, and the metal heteroatom is connected to the non-metal heteroatom via a covalent bond.
[0013] In one embodiment, the non-metallic heteroatom includes at least one of a N atom, a P atom, a S atom, and a B atom.
[0014] In one embodiment, the metal heteroatom includes at least one of a Mo atom, a Co atom, and a Mn atom.
[0015] In one embodiment, the carbon material has active sites, the active sites include carbon surface defects and / or functional groups, and the metal compound is bound to the active sites.
[0016] In one embodiment, the carbon material has a three-dimensional network structure, and the metal compound is bound to the carbon skeleton of the carbon material in the three-dimensional network structure.
[0017] In one embodiment, the mass ratio of the carbon material to the metal compound is 100:(10-150).
[0018] In one embodiment, the doping amount of the non-carbon element heteroatom on the carbon material accounts for 0.1wt%~5wt%.
[0019] In one embodiment, the carbon material includes at least one of carbon nanotubes, carbon fibers, graphene, carbon black, and Ketjen black.
[0020] In one embodiment, the metal compound includes at least one of metal oxide, metal carbide, and metal sulfide.
[0021] In one embodiment, the catalyst is coated on the outer surface of the lithium-rich material to form a coating layer.
[0022] In one embodiment, the D50 particle size of the lithium-rich material is 100 nm to 10 μm.
[0023] In one embodiment, the catalyst accounts for 5wt% to 40wt% of the composite lithium supplement material.
[0024] In a third aspect, the present invention also provides a method for preparing a composite lithium-supplementing material, comprising: mixing and reacting a carbon material and a heteroatom raw material of a non-carbon element to obtain a carbon material doped with heteroatoms of non-carbon elements; mixing and reacting the carbon material and a metal oxide precursor to obtain a catalyst, wherein the metal oxide precursor is converted into a metal compound and grows on the carbon material; and mixing and calcining the catalyst and a lithium-rich material to obtain a composite lithium-supplementing material.
[0025] The preparation method of the composite lithium-supplementing material provided in the present application achieves both electrical conductivity and catalytic ability by doping heteroatoms into the carbon material and converting the metal compound into a metal compound in situ using a metal oxide precursor; and by doping with heteroatoms, the carbon material in the catalyst has higher electrical conductivity and catalytic activity, and the doped carbon material can play a synergistic role with the metal compound to improve the comprehensive performance of the catalyst.
[0026] In a fourth aspect, the present invention further provides a positive electrode material, comprising a positive electrode active material and a lithium supplement material, wherein the lithium supplement material comprises the composite lithium supplement material described in the first aspect, or the positive electrode material comprises the composite lithium supplement material obtained by the preparation method of the composite lithium supplement material described in the second aspect.
[0027] In a fifth aspect, the present invention further provides a secondary battery, comprising a positive electrode, a negative electrode and a separator arranged between the positive electrode and the negative electrode, wherein the positive electrode comprises the positive electrode material described in the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 is a schematic diagram of the appearance of a catalyst according to an embodiment;
[0030] Figure 2 is a schematic diagram of a heteroatom attached to a carbon material according to an embodiment;
[0031] Figure 3 is a SEM image of a catalyst according to an embodiment;
[0032] Figure 4 is a schematic cross-sectional view of a composite lithium supplement material according to an embodiment;
[0033] Figure 5 is a flow chart for preparing a composite lithium supplement material according to an embodiment;
[0034] Figure 6 This is a flow chart for preparing a composite lithium supplement material according to another embodiment. DETAILED DESCRIPTION
[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] It should be noted that when a component is said to be "fixed to" another component, it can be directly on the other component or there can be a central component. When a component is said to be "connected to" another component, it can be directly connected to the other component or there can be a central component at the same time.
[0037] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used in the present invention includes any and all combinations of one or more of the related listed items.
[0038] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0039] The present invention provides a catalyst 10, please refer to Figure 1 and Figure 3 , including a carbon material 11 and a metal compound, wherein the carbon material 11 is doped with heteroatoms of non-carbon elements; and the metal compound 12 is grown on the carbon material 11.
[0040] Specifically, the catalyst 10 acts on the lithium-rich material to catalytically reduce the lithium-desorption potential of the lithium-rich material and improve the conductivity of the lithium-rich material. It is understandable that the catalyst 10 can be mixed with the lithium-rich material and contacted with the lithium-rich material to achieve a catalytic effect. The carbon material 11 in the catalyst 10 can be used to improve the electronic conductivity and ionic conductivity of the lithium-rich material, and the metal compound 12 in the catalyst 10 can be used to reduce the lithium-desorption potential of the lithium-rich material, so that the lithium-rich material can release lithium ions at a lower potential.
[0041] In one embodiment, the carbon material 11 includes at least one of carbon nanotubes, carbon fibers, graphene, carbon black, and Ketjen black. It is understood that the specific form of the carbon material 11 is not limited, including shaped carbon and amorphous carbon. The main purpose of the carbon material 11 is to improve the conductivity of the catalyst 10, thereby improving the conductivity of the composite material after the catalyst 10 is mixed with the lithium-rich material.
[0042] Optionally, the carbon material 11 is doped with heteroatoms of non-carbon elements, and the heteroatoms may be non-metallic heteroatoms or metal heteroatoms. The heteroatoms may be connected to the carbon atoms in the carbon material 11 through chemical bonds. Compared with ordinary carbon materials 11, doping the carbon material 11 with heteroatoms may improve the conductivity of the carbon material 11, thereby improving the conductivity of the catalyst 10. After the catalyst 10 is combined with the lithium-rich material, the conductivity of the lithium-rich material may be improved.
[0043] In addition, the carbon material 11 doped with heteroatoms can also be endowed with catalytic ability and has a high catalytic activity. For example, the boron-doped carbon material 11 has excellent catalytic performance and can be used for oxidation reactions, etc. Moreover, the heteroatom-doped carbon material 11 also has mechanical properties that are superior to those of the pure carbon material 11. For example, boron atom-doped carbon nanotubes are harder, tougher, and have higher compressive strength than pure carbon nanotubes; sulfur atom-doped carbon nanotubes have good toughness and bending modulus, and nitrogen atom-doped carbon nanotubes have high mechanical strength and heat resistance.
[0044] Optionally, the heteroatom-doped carbon material 11 can be prepared by a variety of methods, such as physical grinding and mixing, chemical vapor deposition, arc discharge, laser evaporation, etc.
[0045] In one embodiment, the metal compound 12 includes at least one of metal oxide, metal carbide, and metal sulfide. Optionally, the metal compound 12 may be in a granular structure.
[0046] In a specific embodiment, the metal compound 12 is a metal oxide, and the chemical formula of the metal oxide includes A x O y, A includes at least one of Mo, W, V, Ti, Fe, Co, Ni, Mn, Cr, Cu, and Zn, 1≤x≤3, and 1≤y≤3. For example, the metal compound may include manganese oxide, nickel oxide, cobalt oxide, iron oxide, titanium oxide, molybdenum oxide, vanadium oxide, or niobium oxide.
[0047] Optionally, the metal compound 12 grows on the carbon material 11, wherein the grown metal compound 12 and the carbon material 11 may be connected by a chemical bond, or there may be no chemical bond between the two. Among them, no chemical bond is formed between the metal compound 12 and the carbon material 11, and the metal compound 12 and the carbon material 11 may be connected by intermolecular forces. For example, the metal compound 12 can be formed by an in-situ reaction of a metal oxide precursor. It needs to be explained that the in-situ reaction formation is actually: the metal oxide precursor (such as a hydroxide or a salt) is first combined with the carbon material 11, and then the metal oxide precursor is converted into the metal compound 12 through high-temperature sintering. At this time, the spatial position of the metal compound 12 relative to the metal oxide precursor has not changed.
[0048] In a specific embodiment, taking manganese acetate to prepare MnO as an example, manganese acetate is first adsorbed on the carbon material 11, then hydrolyzed to form Mn(OH)2, and then washed, dried and calcined, and Mn(OH)2 is decomposed into MnO. Of course, in other embodiments, precursors of other metal oxides can also be used.
[0049] The catalyst 10 provided in the present application includes a carbon material 11 and a metal compound 12, wherein the carbon material 11 is doped with heteroatoms, and the metal compound 12 grows on the carbon material 11. The catalyst 10 provided in the present application has the following advantages: 1) The catalyst 10 has both electrical conductivity and catalytic ability. The existing catalytic materials only have catalytic compounds, so the catalytic materials only provide catalytic ability. The present application combines the carbon material 11 and the metal compound 12, and utilizes the high electrical conductivity of the carbon material 11 itself, so that the catalyst 10 has electrical conductivity. After the catalyst 10 is combined with the lithium-rich material, there is no need to add conductive material; 2) The carbon material 11 in the catalyst 10 has higher electrical conductivity and catalytic activity, and is doped with heteroatoms, because doping with heteroatoms can change the electronic structure and chemical properties of the carbon material 11, thereby improving its electrical conductivity, catalytic activity, etc. Compared with the pure carbon material 11 in the prior art, doping The carbon material 11 can play a synergistic role with the metal compound 12 to improve the comprehensive performance of the catalyst 10; 3) The production process of the metal compound 12 directly growing on the carbon material 11 is simple, and the bonding strength between the metal compound 12 and the carbon material 11 is high. Compared with the simply mixed composite catalyst 10 in the prior art, the metal compound 12 provided by the present invention is not easy to fall off from the carbon material 11, so the catalyst 10 has high stability when used; 4) By loading the metal compound 12 on the carbon material 11 by direct growth, a larger loading amount of the metal compound 12 can be obtained on the carbon material 11, because compared with the physical mixing method, the grown metal compound 12 is more likely to form a densely packed structure, and the metal compound 12 is more densely attached, thereby increasing the loading amount of the metal compound 12 on the carbon material 11, so the catalyst 10 provided by the present invention has a higher content of metal compound 12 and a higher catalytic efficiency.
[0050] In one embodiment, the loading amount of the metal compound 12 per unit area of the carbon material 11 is greater than or equal to 10 wt %. Optionally, the loading amount of the metal compound 12 per unit area of the carbon material 11 may be 10 wt %, 12 wt %, 15 wt %, 20 wt %, 30 wt %, 50 wt %, 100 wt %, etc.
[0051] In the catalyst provided by the present invention, the content of metal compound 12 is relatively large (significantly more than the amount of catalyst in the prior art), because the metal compound 12 is grown in situ on the carbon material 11, and compared with the physical mixing method, the grown metal compound 12 has a higher stacking density on the carbon material 11, and the metal compound 12 is more densely attached, so that the content of metal compound 12 per unit area is higher (can exceed 10wt%); and there are a large number of active sites on the carbon material 11, so that the adhesion strength of the metal compound 12 is greater, and the metal compound 12 is not easy to fall off during mixing or transportation, so the loading amount of the metal compound 12 is not easy to reduce.
[0052] When the loading amount of the metal compound 12 per unit area of the carbon material 11 is within the above range, it can be ensured that the catalyst 10 is homogeneous as a whole, the metal compound 12 is evenly distributed on the carbon material 11, and the content of the metal compound 12 is moderate. When the loading amount of the metal compound 12 per unit area of the carbon material 11 is less than the above range, the metal compound 12 in the catalyst 10 is less, and it is difficult to play an effective catalytic role.
[0053] In one embodiment, the present invention provides a composite lithium supplement material, please refer to Figure 4 , including: a lithium-rich material 20 and the catalyst 10 in the above embodiment, wherein the catalyst 10 is combined with the lithium-rich material 20.
[0054] Specifically, the lithium-rich material 20 can be used to supplement lithium. The lithium-rich material 20 can be in a granular form, including a spherical or quasi-spherical form. The lithium-rich material 20 can be a primary particle, or a secondary particle formed by aggregation of primary particles. During the first charging process, the lithium (Li) in the lithium-rich material 20 can be released and migrate to the negative electrode of the battery to offset the irreversible lithium loss caused by the formation of the SEI film, thereby increasing the total capacity and energy density of the battery.
[0055] In some embodiments, the lithium-rich material includes a lithium-supplementing material with a relatively high decomposition voltage, mainly including a lithium-supplementing material with a delithiation potential of more than 4V, such as Li2C2O4 (delithiation potential 4.7V), Li2O (delithiation potential 4.5V), Li2O2 (delithiation potential 4.3V), LiOH (delithiation potential 4.8V), Li4SiO4 (delithiation potential 4.5V), Li3PO4 (delithiation potential exceeding 4V), Li2CO3 (delithiation potential 4.7V), and Li5FeO4 (delithiation potential 4V). These lithium-rich materials have a relatively high capacity, but these lithium-rich materials require a relatively high charging voltage for delithiation, and there is a technical problem of a high platform voltage. At the same time, the relatively high voltage also causes the lithium-supplementing material to generate oxygen when the lithium-ion battery is charged and discharged for the first time, and the generated oxygen is further oxidized to cause the electrolyte to oxidize and decompose, thereby reducing the safety and performance of the lithium-ion battery. These lithium-supplementing materials with higher decomposition voltages are also difficult to compound with conventional positive electrode materials (such as lithium iron phosphate, whose delithiation potential is about 3.5V), which limits the wide application of lithium-supplementing materials. Therefore, the present invention can effectively reduce the decomposition voltage of lithium-rich materials by utilizing the catalytic effect of metal compounds, and further strengthen the catalytic effect of metal compounds through the conductivity of carbon materials, thereby improving the utilization rate of these lithium-rich materials with higher decomposition voltages; in addition, through the binding effect of the active sites on the surface of the carbon material, the carbon material bound to the lithium-rich material strengthens the connection strength between the lithium-rich material and the catalyst, so that the catalyst is not easy to fall off from the lithium-rich material, the catalyst has high stability and a stronger catalytic effect on the lithium-rich material.
[0056] Optionally, the lithium supplement material may also include a binary lithium supplement agent and / or a ternary lithium supplement agent. It is understood that by combining the above catalyst with these lithium supplement agents, it can catalyze the reduction of the decomposition voltage of the lithium supplement agent or improve its conductivity. The chemical formula corresponding to the binary lithium supplement agent is Li x2 M y2 , wherein M is at least one element selected from S, P, N, F, B, O, Se, and Te, 1≤x2≤5, and 0<y2. Binary lithium supplements include but are not limited to at least one selected from Li3N, Li2S, LiF, Li3P, Li2Se, and Li2O.
[0057] Optionally, the chemical formula of the ternary lithium supplement is Li a M b O c, wherein M is at least one element selected from Fe, Ni, Mn, Cu, Zn, Co, Cr, Zr, Sb, Ti, V, Mo, Sn, etc., 1≤a≤8, 0<b, 0<c<7. In a specific embodiment, the lithium-rich material may be Li5FeO4, Li6MnO4, Li6CoO4, Li6ZnO4, Li2NiO2, Li2CuO2, Li2CoO2, Li2MnO2, Li2Ni 0.5 Mn 1.5 O4、Li2Ni d Cu (1-d) At least one of O2 (0<d<1), etc.
[0058] The lithium-rich material 20 mentioned above may be undoped or modified by doping, or may be surface coated, pre-lithiated, etc. In the embodiment of the present invention, when the lithium-rich material 20 is used as the positive electrode active material, the lithium-rich material 20 may also be a combination of the lithium-rich material 20 listed above and conventional positive electrode materials such as lithium iron phosphate and ternary positive electrode materials.
[0059] Optionally, the catalyst 10 and the lithium-rich material 20 can be combined in the following manner: the catalyst 10 is combined on the outer surface of the lithium-rich material 20, for example, the catalyst 10 completely covers or semi-covers the lithium-rich material 20; or, the lithium-rich material 20 is combined on the outer surface of the catalyst 10, for example, the lithium-rich material 20 completely covers or semi-covers the catalyst 10.
[0060] The present invention combines the catalyst 10 provided in the above-mentioned embodiment with the lithium-rich material 20 to obtain a composite lithium-supplementing material, which has the following effects: 1) The lithium-rich material 20 can have a high loading of the catalyst 10. Based on the structure of the catalyst 10, since the content of the metal compound 12 in the catalyst 10 is higher, the composite lithium-supplementing material provided by the present invention has more catalysts 10 in the lithium-supplementing material of the same volume, and the catalytic effect of the catalyst 10 on the lithium-rich material 20 is enhanced, so that the decomposition voltage of the lithium-rich material 20 decreases more significantly; 2) The lithium-rich material 20 and the catalyst 12 are combined to form a composite lithium-supplementing material. The combination of the catalyst 10 and the catalyst 10 is tighter. Since the carbon material 11 in the catalyst 10 can provide a larger specific surface area, the carbon material 11 will have more active sites. The lithium-rich material 20, the carbon material 11 and the metal compound 12 are firmly combined together by using intermolecular forces. The metal compound 12 is not easy to fall off from the carbon material 11, and the catalyst 10 as a whole is not easy to fall off from the lithium-rich material 20. Therefore, in the process of the catalyst 10 catalyzing the lithium-rich material 20, the catalytic effect of the catalyst 10 is enhanced, and the decomposition voltage of the lithium-rich material 20 can be further reduced.
[0061] In one implementation, please refer to Figure 2The heteroatoms of non-carbon elements include non-metallic heteroatoms, and the non-metallic heteroatoms are connected to the carbon atoms of the carbon material 11 through chemical bonds.
[0062] Specifically, the non-metallic heteroatom includes at least one of N atom, P atom, S atom and B atom. Moreover, the non-metallic heteroatom can form a single bond, a double bond or a triple bond with the carbon atom.
[0063] The purpose of doping with non-metallic heteroatoms is to improve the conductivity of the carbon material 11, and to make the carbon material 11 catalytic, thereby improving the comprehensive performance of the carbon material 11. In addition, doping the carbon material 11 with non-metallic heteroatoms can also increase the surface structural defects and surface area of the carbon material 11, exposing more active sites, which is conducive to the subsequent growth of the metal compound 12.
[0064] In one implementation, please refer to Figure 2 Non-carbon heteroatoms also include metal heteroatoms, which are connected to non-metal heteroatoms by covalent bonds.
[0065] Specifically, the metal heteroatom includes at least one of a Mo atom, a Co atom, and a Mn atom. Moreover, the metal heteroatom can form a covalent bond with the non-metal heteroatom.
[0066] The purpose of using metal heteroatom doping modification is to improve the conductivity of carbon material 11, while improving the stability of carbon material 11 in ORR reaction (redox reaction) and providing more active sites; since the catalytic decomposition of lithium-rich materials also involves changes in valence states, which belongs to the category of redox reaction, metal heteroatoms are beneficial to the decomposition of lithium-rich materials; in addition, more active sites are also more conducive to the growth of the later catalyst 10.
[0067] In one embodiment, the carbon material 11 has active sites, which include carbon surface defects and / or functional groups, and the metal compound 12 is bound to the active sites.
[0068] Specifically, based on the above-mentioned embodiment, the metal oxide precursor is first combined with the active site of the carbon material 11, and then reacts in situ at the active site to form the metal compound 12. The active site includes carbon surface defects and / or functional groups, wherein the carbon surface defects come from heteroatom doping, that is, chemical bond defects between some carbon atoms after doping, and metal heteroatom defects; the functional groups come from the carbon material 11 itself or post-processing.
[0069] For example, the provided carbon material 11 originally has some functional groups, which can be oxygen-containing functional groups, such as graphene oxide. Alternatively, the doped carbon material 11 is subjected to surface functionalization treatment so that the surface of the carbon material 11 can have abundant functional groups. In a specific embodiment, the doped carbon material 11 can be placed in an acid solution for cleaning to increase the functional groups and active sites on its surface. Then, the metal oxide precursor is loaded onto the treated carbon material 11.
[0070] Optionally, the functional group is a carboxyl group. The advantage of the carboxyl group is that it is more conducive to the adsorption and loading of the metal compound 12 on the carbon material 11, thereby increasing the loading amount of the catalyst 10.
[0071] By subjecting the carbon material 11 to surface functionalization treatment, the number of its surface functional groups and the adsorption sites of the metal compound 12 can be increased, thereby increasing the loading amount of the metal compound 12 .
[0072] In one embodiment, the carbon material 11 has a three-dimensional network structure, and the metal compound 12 is combined with the carbon skeleton of the carbon material 11 having the three-dimensional network structure.
[0073] Specifically, the carbon material 11 can be a carbon nanotube or a carbon fiber, and a plurality of carbon nanotubes or carbon fibers are interwoven and connected to form a three-dimensional network structure, so each carbon nanotube or carbon fiber constitutes the carbon skeleton mentioned above. Then, at least one carbon nanotube or carbon fiber can be combined with a metal compound 12; it can be understood that the metal compound 12 and the carbon nanotube or carbon fiber form a structure similar to that of grapes and vines.
[0074] The carbon material 11 with a three-dimensional network structure has a larger specific surface area. On the one hand, it is easier to modify, so that the doped heteroatoms can be more evenly distributed on each carbon skeleton; on the other hand, the surface of the carbon material 11 can form more active sites, thereby increasing the loading amount of the metal compound 12 and the connection strength between the two.
[0075] In one embodiment, the carbon material 11 is combined with a part of the outer surface or the entire outer surface of the metal compound 12 , so that the carbon material 11 half-coats or fully coats the metal compound 12 .
[0076] Specifically, based on the above embodiment, the carbon material 11 can also be carbon black or Ketjen black. Most of these carbon materials 11 are in powder form and can be mixed with a metal oxide precursor so that the carbon material 11 is coated on the outer surface of the precursor. Of course, the specific coating style is not limited and can be a semi-coated or fully coated structure.
[0077] In one embodiment, the mass ratio of the carbon material 11 to the metal compound 12 is 100: (10-150). Optionally, the mass ratio of the carbon material 11 to the metal compound 12 may be 100: 10, 100: 20, 100: 30, 100: 40, 100: 50, 100: 60, 100: 70, 100: 80, 100: 90, 100: 100, 100: 110, 100: 120, 100: 130, 100: 140, 100: 150. Optionally, the mass ratio of the carbon material 11 to the metal compound 12 is 100: (10-120), 100: (10-100), 100: (10-80).
[0078] When the mass ratio of the carbon material 11 to the metal compound 12 is within the above range, it can ensure that the catalyst 10 has a high decomposition voltage catalytic ability and a relatively suitable electrical conductivity. When the proportion of the carbon material 11 is greater than the above range, there is too much carbon material 11. Although the conductivity of the catalyst 10 is enhanced, the ability of the catalyst 10 to reduce the catalytic decomposition voltage is weakened. When the catalyst 10 and the lithium-rich material are mixed, the decomposition voltage of the lithium-rich material is limited. When the mass proportion of the metal compound 12 is greater than the above range, the conductivity of the catalyst 10 deteriorates, resulting in the deterioration of the conductivity of the lithium-rich material.
[0079] In one embodiment, the doping amount of heteroatoms on the carbon material 11 is 0.1wt% to 5wt%. Optionally, the doping amount of heteroatoms on the carbon material 11 may be 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, or 5wt%.
[0080] When the proportion of the doping amount of heteroatoms on the carbon material 11 is within the above range, the structural stability of the carbon material 11 can be guaranteed while ensuring the improvement of the electrical conductivity and catalytic activity of the carbon material 11. When the proportion of the doping amount of heteroatoms on the carbon material 11 is less than the above range, the electrical conductivity of the carbon material 11 approaches the undoped state, and the content of the growth-bound metal compound 12 on the carbon material 11 is less, resulting in weaker catalytic activity. When the proportion of the doping amount of heteroatoms on the carbon material 11 is greater than the above range, the chemical bonds of the carbon atoms are mainly connected to the heteroatoms, resulting in a weakening of the connection strength between the carbon atoms of the carbon material 11 and a deterioration of the structural stability of the carbon material 11.
[0081] In one embodiment, there are multiple catalysts 10 , and the multiple catalysts 10 are distributed on the outer surface of the lithium-rich material 20 .
[0082] Specifically, the catalyst 10 and the lithium-rich material 20 can be spherical or quasi-spherical particles, and a plurality of catalysts 10 can be distributed on the outer surface of the lithium-rich material 20. The plurality of catalysts 10 form a discontinuous point distribution on the outer surface of the lithium-rich material 20. The catalysts 10 can be independently distributed on the outer surface of the lithium-rich material 20 to form a discontinuous structure, and the particles of the catalysts 10 are independent of each other.
[0083] It can be understood that, based on the above-mentioned embodiment, the structure of the catalyst 10 can be that the carbon material 11 covers the metal compound 12, so the finally obtained catalyst 10 can also be in a granular form.
[0084] In one embodiment, the catalyst 10 is coated on the outer surface of the lithium-rich material 20 to form a coating layer.
[0085] Specifically, the composite lithium supplement material includes a core and a coating layer, wherein the coating layer is coated on the outer surface of the core; wherein the core includes a lithium-rich material 20, and the coating layer includes a catalyst 10. The catalyst 10 is used to coat the lithium-rich material 20, so that the catalyst 10 is used as an encapsulated coating layer. On the one hand, the catalyst 10 can exert the maximum catalytic effect; on the other hand, the coating layer can reduce the erosion of the lithium-rich material 20 by external water vapor, and reduce the gas production of the material in the core, thereby improving the electrochemical performance of the composite lithium supplement material.
[0086] In one embodiment, the catalyst 10 is a three-dimensional network structure and is coated on the outer surface of the lithium-rich material 20 .
[0087] Specifically, based on the above embodiment, the outer surface of the lithium-rich material 20 is coated with a fishnet-shaped coating layer, and the coating layer is composed of a carbon material 11 with a three-dimensional network structure and a metal compound 12 grown on the carbon material 11.
[0088] In one embodiment, the D50 particle size of the lithium-rich material 20 is 100nm~10μm. Optionally, the D50 particle size of the lithium-rich material 20 can be 100nm, 500nm, 800nm, 1μm, 2μm, 3μm, 5μm, 7μm, 8μm, 9μm, 10μm. Optionally, the D50 particle size of the lithium-rich material 20 is 800nm~10μm, 1μm~10μm, 2μm~10μm.
[0089] When the particle size of the lithium-rich material 20 is within the above range, the catalytic effect of the catalyst 10 on the lithium-rich material 20 can be ensured, the release efficiency of lithium ions can be improved, and the difficulty of preparing the material can be reduced. When the particle size of the lithium-rich material 20 is smaller than the above range, the difficulty of preparing the lithium-rich material 20 increases, and the lithium-rich material 20 is severely agglomerated and difficult to disperse and combine with the catalyst 10. When the particle size of the lithium-rich material 20 is larger than the above range, the catalytic effect of the catalyst 10 on the lithium-rich material 20 is reduced, and the release path of lithium ions is longer, which affects the delithiation efficiency of the material.
[0090] In one embodiment, the mass proportion of the catalyst 10 in the composite lithium supplement material is 5wt%~40wt%. Optionally, the mass proportion of the catalyst 10 in the composite lithium supplement material is 5wt%, 10wt%, 12wt%, 14wt%, 16wt%, 18wt%, 20wt%, 22wt%, 24wt%, 26wt%, 28wt%, 30wt%, 35wt%, 40wt%. Optionally, the mass proportion of the catalyst 10 in the composite lithium supplement material is 10wt%~40wt%, 10wt%~35wt%, 10wt%~30wt%.
[0091] When the mass proportion of the catalyst 10 in the composite lithium-supplementing material is within the above range, the catalytic effect of the catalyst 10 on the lithium-rich material 20 can be ensured, and the lithium ion capacity of the composite lithium-supplementing material can be met. When the mass proportion of the catalyst 10 in the composite lithium-supplementing material is less than the above range, the catalyst 10 is too little, resulting in a poor catalytic effect, and the lithium release voltage of the lithium-rich material 20 is limited. When the mass proportion of the catalyst 10 in the composite lithium-supplementing material is greater than the above range, the catalyst 10 is too much, and since the catalyst 10 does not contribute lithium ions, the lithium capacity is reduced.
[0092] In one embodiment, the present invention also provides a method for preparing a composite lithium supplement material, please refer to Figure 5 ,include:
[0093] Step S10, mixing the carbon material and the non-carbon element heteroatom raw material to obtain the carbon material doped with the non-carbon element heteroatom.
[0094] Step S20, mixing the carbon material and the metal oxide precursor to react to obtain a catalyst, and the metal oxide precursor is converted into a metal compound and grows on the carbon material.
[0095] Step S30, mixing the catalyst and the lithium-rich material together and calcining them to obtain a composite lithium-supplementing material.
[0096] Optionally, in step S10, the type of carbon material may refer to that provided in the above embodiments, which will not be described in detail herein. The heteroatom raw material includes a non-metallic heteroatom raw material and / or a metallic heteroatom raw material.
[0097] Optionally, in step S10, the process method for the mixed reaction of the carbon material and the non-carbon element heteroatom raw material includes but is not limited to physical grinding mixing, chemical vapor deposition, arc discharge, laser evaporation, etc.
[0098] Optionally, in step S20, the metal oxide precursor includes carbonate, sulfate, phosphate, nitrate, organic salt, hydroxide, etc., without specific limitation.
[0099] Optionally, in step S20, the process method for the mixed reaction of the carbon material and the metal oxide precursor includes but is not limited to physical grinding and mixing, high-temperature calcination, chemical vapor deposition or atomic deposition, etc.
[0100] Optionally, the catalyst may be coated on the outer surface of the lithium-rich material to form a coating layer. The type of lithium-rich material may refer to the above embodiment and will not be described in detail here.
[0101] Optionally, the calcination environment in the above steps is an inert atmosphere, and the inert atmosphere includes at least one of nitrogen, argon, helium, etc.
[0102] In one implementation, please refer to Figure 6 The preparation method of the composite lithium supplement material may further specifically include the following steps:
[0103] Step S11, mixing the carbon material and the non-metallic heteroatom raw material to react, to obtain the non-metallic heteroatom doped carbon material.
[0104] Step S12, mixing the carbon material and the metal heteroatom raw material for reaction to obtain a carbon material co-doped with non-metallic heteroatoms and metal heteroatoms, wherein the metal heteroatoms and the non-metallic heteroatoms are connected by covalent bonds.
[0105] Step S21, performing surface functionalization treatment on the carbon material.
[0106] Step S22, mixing the carbon material after the surface functionalization treatment and the metal oxide precursor to react to obtain a catalyst.
[0107] Step S31, mixing the catalyst and the lithium-rich material together and calcining them to obtain a composite lithium-supplementing material.
[0108] Optionally, in step S11, the non-metallic heteroatom raw material may be urea, ammonia water, dopamine hydrochloride, or the like.
[0109] Optionally, in step S11, the carbon material and the non-metallic heteroatom raw material are mixed and reacted, specifically comprising: mixing the carbon material and the non-metallic heteroatom raw material to form a solution, drying to obtain a solid mixture, and grinding the solid mixture to obtain a non-metallic heteroatom-doped carbon material.
[0110] Optionally, in step S12, the metal heteroatom raw material may be an organic metal salt, such as ammonium molybdate, ammonium cobaltate, and the like.
[0111] Optionally, in step S12, the carbon material and the metal heteroatom raw material are mixed and reacted, specifically comprising: mixing the carbon material doped with non-metallic heteroatoms and the metal heteroatom raw material in a solvent, reacting at a high temperature and drying after cooling, and then calcining at a high temperature to obtain a carbon material co-doped with non-metallic heteroatoms and metal heteroatoms.
[0112] Optionally, in step S12, the carbon material and the metal heteroatom raw material may react at high temperature for 6 h to 10 h, and the reaction temperature may be 100° C. to 200° C.
[0113] Optionally, in step S12, the reaction product may be calcined at high temperature for 8 h to 15 h, and the calcination temperature may be 600° C. to 900° C.
[0114] Optionally, in step S21, the carbon material is subjected to surface functionalization treatment, specifically comprising: adding the doped carbon material into a treatment solution, boiling and stirring, and then filtering and drying to obtain a surface functionalized heteroatom-doped carbon material.
[0115] Optionally, in step S21, the treatment liquid may be an acid solution or an alkali solution, including but not limited to nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, oxalic acid, sodium hydroxide, lithium hydroxide, etc.
[0116] Optionally, in step S22, the carbon material after surface functionalization treatment and the metal oxide precursor are mixed and reacted, specifically including: adding the carbon material and the metal oxide precursor into a solvent together, transferring them to a reactor after mixing evenly, reacting at a high temperature and drying after cooling, and then calcining at a high temperature to convert the metal oxide precursor into a metal compound, thereby obtaining a catalyst.
[0117] Optionally, in step S22, the carbon material and the metal oxide precursor may react at high temperature for 8 hours to 15 hours, and the reaction temperature may be 80°C to 200°C.
[0118] Optionally, in step S22, the reaction product may be calcined at high temperature for 3 h to 10 h, and the calcination temperature may be 600° C. to 900° C.
[0119] The preparation method of the catalyst provided in the present application achieves both electrical conductivity and catalytic ability by doping heteroatoms into the carbon material and converting the metal compound into a metal compound in situ using a metal oxide precursor; and by doping with heteroatoms, the carbon material in the catalyst has higher electrical conductivity and catalytic activity, and the doped carbon material can act synergistically with the metal compound to improve the comprehensive performance of the catalyst.
[0120] In addition, the present application also increases the surface functional groups and active sites of the carbon material by acid washing, and then grows a metal compound on the surface of the conductive carbon material, thereby increasing the intermolecular force between the metal compound and the carbon material. Then, it is sintered together with the lithium-rich material and coated on the surface of the lithium-rich material. Since the catalyst already contains a conductive carbon material, there is no need to add additional carbon material. Thus, the metal compound, carbon material and lithium-rich material are firmly combined together, thereby reducing the delithiation potential of the lithium-rich material.
[0121] In one embodiment, the present invention further provides a positive electrode material, the positive electrode material includes a positive electrode active material and a lithium supplement material. The lithium supplement material includes the composite lithium supplement material provided in the above embodiment. Optionally, the positive electrode active material can be a phosphate positive electrode active material and a ternary positive electrode active material, and in a specific embodiment, includes one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, lithium fluorinated vanadium phosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.
[0122] In one embodiment, the content of the composite lithium supplement material in the positive electrode material can be controlled at 1% to 6% of the mass of the positive electrode active material. This ratio can just make up for the loss of active lithium in the battery during the first charging process. If the amount of composite lithium supplement material added to the positive electrode material is too low, the active lithium lost in the positive electrode active material cannot be fully replenished, which is not conducive to improving the energy density and capacity retention rate of the battery. If the amount of composite lithium supplement material added to the positive electrode active material is too high, the original reversible capacity will be occupied and the cost will be increased. In some specific embodiments, in the positive electrode material, the mass percentage of the composite lithium supplement material can be 1%, 2%, 4%, 6%, etc.
[0123] In one embodiment, the present invention further provides a positive electrode plate, the positive electrode plate includes a current collector and an active material layer disposed on the current collector, the active material layer includes the composite lithium supplement material of any one of the above embodiments. Or the active material layer includes the composite lithium supplement material obtained by the preparation method of the composite lithium supplement material in the above embodiments.
[0124] In one embodiment, the positive electrode sheet includes a positive electrode current collector, and the positive electrode current collector has a positive electrode active layer, and the positive electrode active layer includes components such as positive electrode active materials, composite lithium supplement materials, conductive agents, and binders. The present invention does not specifically limit these materials, and suitable materials can be selected according to actual application requirements. The positive electrode current collector includes but is not limited to any one of copper foil and aluminum foil. The conductive agent includes one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60 and carbon nanotubes, and the content of the conductive agent in the positive electrode active layer is 3wt%~5wt%. The types of binders include polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan and chitosan derivatives, and the content of the binder in the positive electrode active layer is 2wt%~4wt%.
[0125] In one embodiment, the present invention further provides a secondary battery, comprising a negative electrode sheet, a separator and the positive electrode sheet mentioned above. The positive electrode sheet comprises the composite positive electrode material mentioned above.
[0126] The technical solution of the present invention is described in detail below through specific embodiments.
[0127] Example 1
[0128] This embodiment provides a catalyst and a composite lithium supplement material.
[0129] The composite lithium supplement material includes a catalyst (MnO@CNT) and a lithium-rich material (Li2C2O4), and the catalyst is coated on the outer surface of the lithium-rich material. Among them, CNT (carbon nanotube) is doped with N atoms and Mo atoms, and the N atoms are connected to the C atoms of CNT through chemical bonds, and the N atoms are connected to the Mo atoms through covalent bonds.
[0130] Among them, the doping amount of N atoms and Mo atoms on CNT accounts for 2wt%; the mass ratio of CNT and MnO is 100:66.7; the loading amount of MnO on CNT is 40wt%; the D50 particle size of the lithium-rich material is 3μm; the thickness of the coating layer is 100nm; the mass ratio of the catalyst when mixed with the lithium-rich material is 20wt%.
[0131] The preparation method of the composite catalyst and the composite lithium supplement material comprises the following steps:
[0132] (1) 40 ml of ethanol was added to 2.0 g of CNT and 6.0 g of urea to form a mixed solution. The sample was then ground at 600 rpm for 4 h to obtain N-atom-doped CNT.
[0133] (2) Dissolve 2.0 g of ammonium molybdate and 2.0 g of N-doped CNTs in 30 ml of deionized water, stir evenly, transfer to a reactor and maintain at 160 °C for 8 h. Cool to room temperature, take out, wash with deionized water, dry, and then heat at 800 °C in a tube furnace under an inert atmosphere for 10 h to obtain Mo-doped (modified) N-doped CNTs.
[0134] (3) Disperse 2.0 g of doped CNTs in 40 ml of 60% concentrated nitric acid, stir magnetically and boil for 2 h, filter, wash and dry to obtain surface functionalized doped CNTs.
[0135] (4) Add 1 g of surface functionalized doped CNT and 10 g of manganese acetate tetrahydrate to a mixed solution of 30 ml of deionized water and 20 ml of ethanol, mix well and transfer to a reactor, maintain at 120 °C for 12 h, return to room temperature, wash with deionized water and dry to obtain a catalyst precursor loaded on carbon.
[0136] (5) The obtained CNT loaded with catalyst precursor was placed in a tubular furnace and maintained at 600 °C for 5 h under an inert atmosphere to obtain MnO@CNT.
[0137] (6) Then, the obtained 0.15 g MnO@CNT and 0.85 g Li2C2O4 were mixed by grinding and homogenizing, and then maintained at 400 °C for 5 h under an inert atmosphere to obtain a composite lithium supplement material.
[0138] Example 2
[0139] This embodiment provides a catalyst and a composite lithium supplement material.
[0140] The composite lithium supplement material includes a catalyst (MnO@CNT) and a lithium-rich material (Li2C2O4), and the catalyst is coated on the outer surface of the lithium-rich material. Among them, CNT (carbon nanotube) is only doped with N atoms, and the N atoms are connected to the C atoms of CNT through chemical bonds.
[0141] Among them, the doping amount of N atoms on CNT accounts for 0.8wt%; the mass ratio of CNT and MnO is 100:51.5, and the loading amount of MnO on CNT is 34wt%; the D50 particle size of the lithium-rich material is 3μm; the thickness of the coating layer is 180nm; the mass proportion of the catalyst when mixed with the lithium-rich material is 20wt%.
[0142] The difference between the preparation method of Example 2 and Example 1 is that only N element is doped on the CNT, and no metal element is doped.
[0143] Example 3
[0144] This embodiment provides a catalyst and a composite lithium supplement material.
[0145] The composite lithium supplement material includes a catalyst (MnO@CNT) and a lithium-rich material (Li2C2O4), and the catalyst is coated on the outer surface of the lithium-rich material. Among them, Mo atoms are doped in CNT (carbon nanotubes), and the Mo atoms are connected to the C atoms of CNT through chemical bonds.
[0146] Among them, the doping amount of Mo atoms on CNT accounts for 1.2wt%; the mass ratio of CNT and MnO is 100:42.9, and the loading amount of MnO on CNT is 30wt%; the D50 particle size of the lithium-rich material is 3μm; the thickness of the coating layer is 200nm; the mass proportion of the catalyst when mixed with the lithium-rich material is 20wt%.
[0147] The difference between the preparation method of Example 3 and Example 1 is that only Mo element is doped on the CNT, and N element is not doped.
[0148] Example 4
[0149] This embodiment provides a catalyst and a composite lithium supplement material.
[0150] The composite lithium supplement material includes a catalyst (MnO@CNT) and a lithium-rich material (Li2C2O4), and the catalyst is coated on the outer surface of the lithium-rich material. Among them, CNT (carbon nanotube) is doped with N atoms and Mo atoms, and the N atoms are connected to the C atoms of CNT through chemical bonds, and the N atoms are connected to the Mo atoms through covalent bonds.
[0151] Among them, the doping amount of N atoms and Mo atoms on CNT accounts for 1.3wt%; the mass ratio of CNT and MnO is 100:25, and the loading amount of MnO on CNT is 20wt%; the D50 particle size of the lithium-rich material is 3μm; the thickness of the coating layer is 200nm; the mass proportion of the catalyst when mixed with the lithium-rich material is 20wt%.
[0152] The difference between the preparation method of Example 4 and Example 1 is that the CNT is not acid-washed.
[0153] Example 5
[0154] This embodiment provides a catalyst and a composite lithium supplement material.
[0155] The composite lithium supplement material includes a catalyst (MnO@CNT) and a lithium-rich material (Li2C2O4), and the catalyst is coated on the outer surface of the lithium-rich material. Among them, CNT (carbon nanotube) is doped with N atoms and Mo atoms, and the N atoms are connected to the C atoms of CNT through chemical bonds, and the N atoms are connected to the Mo atoms through covalent bonds.
[0156] Among them, the doping amount of N atoms and Mo atoms on CNT accounts for 2wt%; the mass ratio of CNT and NiO is 100:47.1, and the loading amount of NiO on CNT is 32wt%; the D50 particle size of the lithium-rich material is 3μm; the thickness of the coating layer is 160nm; the mass proportion of the catalyst when mixed with the lithium-rich material is 20wt%.
[0157] The difference between the preparation method of Example 5 and that of Example 1 is that the metal compound in the catalyst is changed from MnO to NiO.
[0158] Example 6
[0159] This embodiment provides a catalyst and a composite lithium supplement material.
[0160] The composite lithium supplement material includes a catalyst (MnO@CNT) and a lithium-rich material (Li2CO3), and the catalyst is coated on the outer surface of the lithium-rich material. Among them, CNT (carbon nanotube) is doped with N atoms and Mo atoms, N atoms are connected to CNT C atoms through chemical bonds, and N atoms are connected to Mo atoms through covalent bonds.
[0161] Among them, the doping amount of N atoms and Mo atoms on CNT accounts for 2wt%; the mass ratio of CNT and MnO is 100:66.7; the loading amount of MnO on CNT is 40wt%; the D50 particle size of the lithium-rich material is 5μm; the thickness of the coating layer is 140nm; the mass proportion of the catalyst when mixed with the lithium-rich material is 20wt%.
[0162] The difference between the preparation method of Example 6 and Example 1 is that lithium oxalate as the lithium-rich material is replaced by lithium carbonate as the lithium-rich material.
[0163] Comparative Example 1
[0164] This comparative example provides a lithium-rich material (Li2C2O4).
[0165] Comparative Example 2
[0166] This comparative example provides a lithium-rich material (Li2CO3).
[0167] Comparative Example 3
[0168] This comparative example provides a composite lithium supplement material, which includes MnO and Li2C2O4, and MnO and Li2C2O4 are simply mixed.
[0169] Comparative Example 4
[0170] This comparative example provides a composite lithium supplement material, which includes CNT and Li2C2O4, and CNT and Li2C2O4 are simply mixed.
[0171] Comparative Example 5
[0172] This comparative example provides a composite lithium supplement material, which includes MnO, CNT and Li2C2O4, and MnO, CNT and Li2C2O4 are simply mixed.
[0173] The composite lithium supplement material provided in the above-mentioned Examples 1-6 and the composite lithium supplement material provided in Comparative Examples 1-5 are respectively assembled into a positive electrode sheet and a lithium ion battery according to the following method:
[0174] Positive electrode sheet: The composite lithium supplement material, SP and PVDF are mixed in a mass ratio of 90:4:6 to form a positive electrode slurry, the positive electrode slurry is coated on the surface of aluminum foil, vacuum dried at 110°C overnight, and rolled to obtain a positive electrode sheet;
[0175] Negative electrode: lithium sheet;
[0176] Electrolyte: Ethylene carbonate and ethyl methyl carbonate were mixed in a volume ratio of 3:7, and LiPF6 was added to form an electrolyte, and the concentration of LiPF6 was 1 mol / L;
[0177] Diaphragm: Polypropylene microporous separator;
[0178] Lithium-ion battery assembly: Assemble button-type lithium-ion full batteries in an inert atmosphere glove box in the order of negative electrode sheet - separator - electrolyte - positive electrode sheet.
[0179] The electrochemical performance of each lithium-ion battery assembled in the above lithium-ion battery embodiment was tested under the following test conditions:
[0180] The battery was charged at a rate of 0.1C, with a cut-off voltage of 4.7V; constant voltage charging was performed at a cut-off voltage of 4.7V. After the charging process was completed, the battery was left to stand for 10 minutes, and then discharged at a rate of 0.1C, with a cut-off voltage of 2.5V.
[0181] Test of electronic conductivity: The resistivity of the positive electrode lithium supplement material in each embodiment and comparative example was calculated by a four-probe method, and the electronic conductivity was obtained by taking the inverse of the resistivity.
[0182] The test results of the above composite lithium supplement material and lithium battery are shown in the following Table 1:
[0183] Table 1. Test results of embodiments and comparative examples
[0184] Performance Parameters Implementation Group First charge specific capacity (mAh / g) <![CDATA[Charge voltage plateau (V vs. Li + / Li)]]> Electronic conductivity (S / m) Example 1 505 4.1 <![CDATA[3.42*10 -5 ]]> Example 2 500 4.12 <![CDATA[3.25*10 -5 ]]> Example 3 492 4.15 <![CDATA[3.11*10 -5 ]]> Example 4 477 4.23 <![CDATA[2.13*10 -5 ]]> Example 5 501 4.13 <![CDATA[3.2*10 -5 ]]> Example 6 365 4.43 <![CDATA[3.63*10 -5 ]]> Comparative Example 1 231 4.65 <![CDATA[1.8*10 -7 ]]> Comparative Example 2 157 4.6 <![CDATA[3.6*10 -7 ]]> Comparative Example 3 423 4.35 <![CDATA[0.8*10 -5 ]]> Comparative Example 4 356 4.41 <![CDATA[2.8*10 -5 ]]> Comparative Example 5 443 4.32 <![CDATA[1.97*10 -5 ]]>
[0185] From the test results of Example 1 and Comparative Example 1 in Table 1, it can be seen that the initial charge specific capacity and electronic conductivity of the composite lithium supplement material prepared in Example 1 are much higher than those of the common lithium oxalate in Comparative Example 1, and the charging voltage platform of the composite lithium supplement material in Example 1 is lower than that of the common lithium oxalate in Comparative Example 1. This shows that the solution provided by the present invention can improve the electronic conductivity of the material on the basis of reducing the charging voltage platform of the lithium-rich material, so that the capacity of the material can be fully released and the matching degree of battery use can be improved. Therefore, the electrochemical performance of the composite lithium supplement material provided by the present invention is much higher than that of the existing common lithium-rich material.
[0186] From the test results of Examples 1 to 3 in Table 1, it can be seen that the performance of the composite lithium supplement material can be further improved by doping non-carbon heteroatoms (metal heteroatoms or non-metal heteroatoms) in the carbon material. In Example 2, no metal element (Mo atom) is doped, and in Example 3, no non-metal element (N atom) is doped, so the active sites on the carbon materials of Examples 2 and 3 are less than those of Example 1, and the stability of the carbon material of Example 2 in the ORR reaction (redox reaction) is weaker than that of Example 1, so the catalysts in Examples 2 and 3 have less metal oxide loading than that of Example 1, and the activity of catalyzing the redox reaction is also weaker than that of Example 1.
[0187] From the test results of Example 1 and Example 4 in Table 1, it can be seen that acid washing has an impact on the performance of the catalyst. Because acid washing can increase the surface functional groups and active sites of the carbon material, and then grow metal compounds on the surface of the carbon material, increasing the intermolecular force between the metal compound and the carbon material. Therefore, the catalytic effect of the catalyst is stronger, the catalyst loading in the obtained composite lithium supplement material is higher, the corresponding first charge specific capacity is higher, the voltage platform is lower, and the electronic conductivity is also higher.
[0188] From the test results of Example 1, Example 5 and Example 6 in Table 1, it can be seen that different metal oxides as catalysts and different lithium-rich materials are all suitable for this improvement method. By comparing Example 1 and Example 5, it can be seen that different metal compounds as catalysts can reduce the lithium delithiation potential of lithium-rich materials and increase the first charge specific capacity and electronic conductivity; from the lithium-ion battery performance of Comparative Example 1 and Example 6, it can be seen that this method is applicable to different lithium-rich material systems.
[0189] From the test results of Example 1 and Comparative Example 1, and Example 6 and Comparative Example 2 in Table 1, it can be seen that whether Li2C2O4 is used as the lithium-rich material or Li2CO3 is used as the lithium-rich material, the performance is significantly improved after being doped with a high-load catalyst grown on the carbon surface, which proves the feasibility of element doping and acid washing of CNTs and growing metal compounds on their surface as catalysts.
[0190] By comparing the lithium-ion battery performances of Example 1, Comparative Example 3, Comparative Example 4 and Comparative Example 5, it can be seen that if the metal compound catalyst, the conductive carbon material and the lithium-rich material are simply mixed together mechanically, the bonding between the three is not strong enough, so even though the components are mixed consistently, the performance is not as good as that of the catalyst grown on the carbon surface. This illustrates the necessity of doping and modifying the carbon material and growing the catalyst on its surface.
[0191] In the description of the embodiments of the present invention, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship described in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0192] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope covered by the present invention.
Claims
1. A composite lithium supplement material, characterized in that: It comprises a lithium-rich material and a catalyst; the catalyst comprises a carbon material and a metal compound, the carbon material is doped with heteroatoms of non-carbon elements, and the metal compound grows on the carbon material; the heteroatoms of non-carbon elements comprise non-metallic heteroatoms and metal heteroatoms, the non-metallic heteroatoms are chemically bonded to the carbon atoms of the carbon material, and the metal heteroatoms are covalently bonded to the non-metallic heteroatoms; the catalyst is coated on the outer surface of the lithium-rich material to form a coating layer; the D50 particle size of the lithium-rich material is 800nm~10μm; The non-metallic heteroatoms include at least one of N atoms, P atoms, S atoms, and B atoms; the metal heteroatoms include at least one of Mo atoms, Co atoms, and Mn atoms; the carbon material includes at least one of carbon nanotubes, carbon fibers, graphene, carbon black, and Ketjen black; the metal compound includes at least one of metal oxides, metal carbides, and metal sulfides.
2. The composite lithium supplement material according to claim 1, characterized in that: The surface of the carbon material has active sites, the active sites include carbon surface defects and / or functional groups, and the metal compound is bound to the active sites; and / or The carbon material has a carbon skeleton with a three-dimensional network structure, and the metal compound is bound to the carbon skeleton; The mass ratio of the carbon material to the metal compound is 100:(10-150); The doping amount of the non-carbon element heteroatom on the carbon material accounts for 0.1wt%~5wt%.
3. The composite lithium supplement material according to claim 1, characterized in that: The catalyst accounts for 5wt% to 40wt% of the composite lithium supplement material.
4. A method for preparing a composite lithium supplement material, characterized in that: include: The carbon material and the non-carbon element heteroatom raw material are mixed and reacted to obtain the carbon material doped with the non-carbon element heteroatom; The carbon material and the metal compound precursor are mixed and reacted to convert the metal compound precursor into a metal compound and grow it on the carbon material to obtain a catalyst; The catalyst and the lithium-rich material are mixed together and calcined to obtain a composite lithium-supplementing material; The non-carbon element heteroatom includes a non-metallic heteroatom and a metal heteroatom, the non-metallic heteroatom is connected to the carbon atom of the carbon material by a chemical bond, and the metal heteroatom is connected to the non-metallic heteroatom by a covalent bond; the catalyst is coated on the outer surface of the lithium-rich material to form a coating layer; the D50 particle size of the lithium-rich material is 800nm~10μm; The non-metallic heteroatoms include at least one of N atoms, P atoms, S atoms, and B atoms; the metal heteroatoms include at least one of Mo atoms, Co atoms, and Mn atoms; the carbon material includes at least one of carbon nanotubes, carbon fibers, graphene, carbon black, and Ketjen black; the metal compound includes at least one of metal oxides, metal carbides, and metal sulfides.
5. A positive electrode material, characterized in that The positive electrode material includes an active material and a lithium supplement material, and the lithium supplement material includes the composite lithium supplement material according to any one of claims 1 to 3, or includes the composite lithium supplement material obtained by the preparation method of the composite lithium supplement material according to claim 4.
6. A secondary battery, characterized in that: The invention comprises a positive electrode, a negative electrode and a separator arranged between the positive electrode and the negative electrode, wherein the positive electrode comprises the positive electrode material as claimed in claim 5.