A kind of lignocellulose full-component hydrogel and its preparation method and application
Through steam explosion pretreatment and freeze-thaw treatment, the lignocellulose full-component hydrogel is formed, which solves the problems of complicated operation and the use of toxic chemical reagents in the prior art, and achieves efficient and environmentally friendly hydrogel preparation and excellent mechanical properties. , suitable for sand fixing agent.
Patent Information
- Application Number
- CN202410598974.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-15
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-05-15
AI Technical Summary
The existing lignocellulose-based hydrogel preparation methods are complicated to operate and require the use of toxic chemical reagents, which limits its industrial production and large-scale utilization, and has uneven performance.
The steam explosion pretreatment destroys the dense structure of lignocellulose, combined with polyvinyl alcohol for freeze-thawing treatment, forming a full-component hydrogel of lignocellulose. The process is simple and fast, and no crosslinking agents and initiators are used to form excellent mechanics. Performance three-dimensional network structure.
It realizes efficient preparation of lignocellulose full-component hydrogel, excellent mechanical properties, biodegradable, suitable for sand fixing agents, environmentally friendly, and without residues.
Smart Images

Figure CN118165299B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lignocellulose bio-based materials, and relates to a lignocellulose full-component hydrogel, and in particular to a lignocellulose full-component hydrogel and a preparation method and application thereof. Background Art
[0002] Hydrogel is a type of polymer with a three-dimensional network structure. It can absorb a large amount of water and swell in water, and after swelling, it can continue to maintain its original structure without being dissolved. Low-cost natural polymer cross-linked hydrogel mainly grafts hydrophilic monomers onto the molecular chain of natural polymer materials through grafting polymerization reaction, and has excellent water absorption performance. The introduction of natural polymer materials not only changes the chemical structure of hydrogels, but also improves their biodegradability, and the impact of the product on the environment after disposal is small. As the most widely existing natural polymer material in nature, lignocellulose has great application potential, especially agricultural waste and food processing residues. Using it as a raw material for gelation can not only improve its utilization value but also solve the problem of gel production costs.
[0003] At present, the synthesis of lignocellulose-based hydrogels still faces a series of problems. The dense structure of lignocellulose itself leads to poor reaction accessibility, and the strong heterogeneity leads to uneven performance of hydrogel products. At present, the preparation of lignocellulose hydrogels is mostly limited to the use of a single component and requires chemical modification to improve the solubility of the component. Both the separation and purification of the components and the chemical modification operation steps are not conducive to the large-scale conversion of lignocellulose. For example, CN105504315A discloses a preparation method and application of a straw-based hydrogel, wherein the straw is first made into an aqueous solution containing cellulose, hemicellulose and lignin, and then an initiator is used to generate free radicals, acrylic acid is grafted, and then a cross-linking agent is used to obtain a hydrogel with a three-dimensional structure; CN110975832A discloses a straw-based hydrogel adsorbent for efficiently removing heavy metal ions and a preparation method thereof, wherein the straw is modified, and an acrylonitrile polymer is grafted on its surface using an atom transfer radical polymerization process to prepare a straw-based hydrogel. The above methods all have the problem of complicated operation and require the use of toxic chemical products such as initiators and cross-linking agents, which limits their industrial production and large-scale utilization.
[0004] Therefore, it is necessary to provide a method for efficiently utilizing all components of lignocellulosic biomass and preparing hydrogels simply and quickly. Summary of the invention
[0005] The purpose of the present invention is to provide a lignocellulose full-component hydrogel and a preparation method and application thereof. The hydrogel is prepared by using the lignocellulose full-component as raw materials. The process is simple and fast, no toxic chemical reagents are used, and the prepared hydrogel has excellent mechanical properties and can be used as a sand fixation agent.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing a hydrogel by steam explosion pretreatment of all components of lignocellulose, the method comprising the following steps:
[0008] (1) subjecting the lignocellulose raw material to steam explosion treatment and then crushing the raw material to obtain a crushed lignocellulose raw material;
[0009] (2) The crushed lignocellulose raw material obtained in step (1) is mixed with the polyvinyl alcohol solution and then subjected to freeze-thaw treatment to obtain a hydrogel.
[0010] The method provided by the present invention uses steam explosion pretreatment as a means to produce a full-component lignocellulose-based hydrogel. The steam explosion pretreatment can destroy the dense structure of lignocellulose. Under the activation effect of the steam explosion pretreatment, the structure of lignocellulose is loosened, the chemical components are partially degraded, and the functional groups that can be cross-linked with the hydroxyl groups in PVA, such as alcoholic hydroxyl groups, phenolic hydroxyl groups, and carboxyl groups, are exposed, and can interact with PVA molecules through hydrogen bond interactions. The obtained hydrogel obtains a dense three-dimensional network structure due to the addition of cellulose, hemicellulose and lignin, thereby having significantly improved mechanical properties. During the process, no other separation, purification or modification operations are required for the lignocellulose biomass raw materials, and no toxic organic solvents such as cross-linking agents and initiators are used. The environmental burden is small, there is no residue, the process is short, the process is green and efficient, simple and fast, and the process is highly universal.
[0011] Preferably, the lignocellulosic raw material in step (1) comprises any one of agricultural and forestry wastes, food processing byproducts, wood or bamboo, or a combination of at least two of them.
[0012] Exemplarily, the agricultural and forestry waste includes straw.
[0013] Exemplarily, the food processing by-products include cereal bran and / or chaff.
[0014] Preferably, before the steam explosion treatment in step (1), the lignocellulosic raw material is pre-impregnated.
[0015] Preferably, the pre-soaking medium comprises water or a soluble alkaline salt solution.
[0016] Preferably, the soluble alkaline salt comprises a bicarbonate salt.
[0017] Preferably, the moisture content of the pre-impregnated lignocellulosic raw material is 30-66%, for example, it can be 30%, 35%, 40%, 45%, 50%, 52%, 54%, 55%, 56%, 58%, 60%, 62%, 64%, 65% or 66%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] Preferably, the pressure of the steam explosion treatment in step (1) is 0.8-1.5 MPa, for example, 0.8 MPa, 0.9 MPa, 1.0 MPa, 1.1 MPa, 1.2 MPa, 1.3 MPa, 1.4 MPa or 1.5 MPa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, the pressure holding time of the steam explosion treatment in step (1) is 5-20 min, for example, 5 min, 8 min, 10 min, 12 min, 15 min, 18 min or 20 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0020] Preferably, the temperature of the steam explosion treatment in step (1) is 170-200°C, for example, 170°C, 175°C, 180°C, 185°C, 190°C, 195°C or 200°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0021] Preferably, the particle size of the crushed lignocellulosic raw material in step (1) is 40-200 mesh, for example, 40 mesh, 50 mesh, 60 mesh, 80 mesh, 100 mesh, 120 mesh, 140 mesh, 150 mesh, 160 mesh, 180 mesh or 200 mesh, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0022] The type of polyvinyl alcohol in step (2) can be any PVA raw material available to those skilled in the art.
[0023] Preferably, the degree of polymerization of the polyvinyl alcohol in step (2) is 1700.
[0024] Preferably, the alcoholysis degree of the polyvinyl alcohol in step (2) is in the range of 87-99%, for example, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or 99%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0025] Preferably, the model of the polyvinyl alcohol includes any one of PVA1799, PVA1788 or PVA1750±50, or a combination of at least two of them. Typical but non-limiting combinations include a combination of PVA1799 and PVA1788, a combination of PVA1788 and PVA1750±50, a combination of PVA1799 and PVA1750±50, or a combination of PVA1799, PVA1788 and PVA1750±50.
[0026] Preferably, the concentration of the polyvinyl alcohol solution in step (2) is 1-20wt%, for example, 1wt%, 3wt%, 5wt%, 8wt%, 10wt%, 12wt%, 15wt%, 18wt% or 20wt%, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0027] Preferably, the polyvinyl alcohol solution in step (2) is prepared by dispersing polyvinyl alcohol powder in water and then heating to dissolve it.
[0028] Preferably, the heating temperature is 90-95°C, for example, 90°C, 91°C, 92°C, 93°C, 94°C or 95°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] Preferably, the mass ratio of the lignocellulosic raw material to polyvinyl alcohol is 1-100%, for example, 1%, 5%, 10%, 30%, 50%, 80% or 100%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 20-50%.
[0030] When the mass ratio of cellulose raw material to polyvinyl alcohol is less than 1%, the cellulose substrate cannot play a reinforcing role on the hydrogel. When the mass ratio of cellulose to polyvinyl alcohol is greater than 100%, the water absorption of cellulose causes the system to be unable to disperse evenly, and thus a homogeneous gel structure cannot be formed through freeze-thaw.
[0031] Preferably, stirring is performed during the mixing.
[0032] Preferably, the stirring speed is 150-450 rpm, for example, it can be 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm or 450 rpm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the stirring time is 1-10 min, for example, 1 min, 3 min, 5 min, 8 min or 10 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0034] Preferably, the freezing of the freeze-thaw treatment is carried out below 0°C, for example, -4°C, -18°C, -50°C or -80°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] Exemplarily, the freezing method of the freeze-thaw treatment includes liquid nitrogen freezing and / or refrigerator freezing.
[0036] Exemplarily, the thawing method of the freeze-thaw treatment includes natural thawing at room temperature.
[0037] In a second aspect, the present invention provides a lignocellulose full-component hydrogel, wherein the lignocellulose full-component hydrogel is prepared by the method described in the first aspect.
[0038] The hydrogel provided by the present invention forms a three-dimensional network structure by cross-linking cellulose, hemicellulose and lignin in the lignocellulose raw material with polyvinyl alcohol, which significantly improves the mechanical properties of the hydrogel, and its tensile strength can reach 329.75 kPa; and the components use biomass as raw materials, do not contain toxic solvents such as cross-linking agents and initiators, and are biodegradable; it has excellent performance as a sand-fixing agent and is environmentally friendly.
[0039] In a third aspect, the present invention provides an application of the lignocellulose full-component hydrogel described in the second aspect, wherein the lignocellulose full-component hydrogel is used as a sand-fixing agent.
[0040] The hydrogel is crushed and dispersed, then sandblasted on the sand surface. After natural air drying, it forms a crust, which effectively fixes the sand particles. The hydrogel contains a large amount of biomass raw materials, which are biodegradable and can be decomposed in the natural environment without causing pollution. After the biomass raw materials in the hydrogel are decomposed into organic matter, it is expected to improve the desert environment.
[0041] Preferably, the method for using the hydrogel as a sand-fixing agent comprises dispersing the hydrogel in water for use.
[0042] Preferably, the dispersion is carried out in a mass ratio of hydrogel to water of 1:(1-10), for example, 1:1, 1:3, 1:5, 1:8 or 1:10, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0043] Compared with the prior art, the present invention has the following beneficial effects:
[0044] The method provided by the present invention uses all components of lignocellulose as raw materials for steam explosion pretreatment, and forms a hydrogel by crosslinking with polyvinyl alcohol through freeze-thaw treatment. The obtained hydrogel has excellent mechanical properties, and its tensile strength can reach 329.75 kPa, and its tensile strain can reach more than 380%. Moreover, the components use biomass as raw materials, do not contain toxic solvents such as crosslinking agents and initiators, and are biodegradable. The DPPH free radical scavenging rate in 30 minutes reaches 77.23%. It has excellent performance as a sand fixation agent and is environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 1 is the stress-strain curve of the hydrogel provided in Example 1 and Comparative Examples 1 and 2;
[0046] Figure 2 is the stress-strain curve of the hydrogel provided in Example 1, Example 4 and Example 5;
[0047] Figure 3 is a bar graph of DPPH free radical scavenging rate of the hydrogels provided in Example 1 and Comparative Examples 1 and 2;
[0048] Figure 4 It is a wind erosion rate curve diagram of the hydrogel provided in Example 1 and Comparative Example 3. DETAILED DESCRIPTION
[0049] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0050] Example 1
[0051] This embodiment provides a method for preparing a hydrogel by steam explosion pretreatment of all components of lignocellulose, the method comprising the following steps:
[0052] (1) The corn stalks were rehydrated to a moisture content of 30%, chopped, and placed in a steam explosion tank. The pressure was set to 1.0 MPa, and the steam explosion temperature was 185°C. After the explosion, the corn stalks were dried and placed in a grinder for crushing. The corn stalks were sieved with a 60-mesh sieve to obtain steam-exploded corn stalk powder.
[0053] (2) Add 20 parts by mass of 10% PVA1799 solution to 1 part by mass of steam-exploded corn straw powder, and blend them at 95°C and 150 rpm for 10 min to obtain a steam-exploded corn straw hydrogel precursor. Then, the hydrogel precursor was placed in a mold and placed in a refrigerator, frozen at -18°C for 12 h, and then thawed at room temperature to obtain a lignocellulose-based hydrogel of steam-exploded corn straw.
[0054] Example 2
[0055] This embodiment provides a method for preparing a hydrogel by steam explosion pretreatment of all components of lignocellulose, the method comprising the following steps:
[0056] (1) Mix wheat bran with 10% baking soda until the moisture content of the wheat bran reaches 30%, then put it into a steam explosion tank, set the parameter pressure to 0.8 MPa, process for 5 minutes, and the temperature of the steam explosion process is 180°C. After explosion, dry it naturally, put it into a grinder, and sieve it with a 60-mesh screen to obtain steam-exploded wheat bran powder;
[0057] (2) Take 1 part by mass of steam-exploded wheat bran, add 10 parts by mass of 20% PVA1788 solution, blend at 90°C and 300 rpm for 5 min to obtain a steam-exploded corn straw hydrogel precursor, then place the hydrogel precursor in a mold and put it in a refrigerator, freeze it at -80°C for 3 h, and then thaw it at room temperature to obtain a lignocellulose-based hydrogel containing all components of the steam-exploded corn straw.
[0058] Example 3
[0059] This embodiment provides a method for preparing a hydrogel by steam explosion pretreatment of all components of lignocellulose, the method comprising the following steps:
[0060] (1) Rehydrate the poplar wood powder, control its water content to 60%, and then put it into a steam explosion tank. Set the parameter pressure to 1.5 MPa, treat it for 20 minutes, and the temperature of the steam explosion treatment is 200°C. After the explosion, dry it naturally, put it into a grinder, and sieve it with a 60-mesh screen to obtain steam-exploded poplar wood powder;
[0061] (2) Take 1 mass part of steam-exploded poplar wood powder, add 20 mass parts of PVA1750±50 solution with a concentration of 15%, and blend them at 93°C and a stirring speed of 450 rpm for 20 min to obtain a steam-exploded corn straw hydrogel precursor. Then, the hydrogel precursor is placed in a mold and quickly frozen by pouring liquid nitrogen, and then thawed at room temperature to obtain a lignocellulose-based hydrogel of the steam-exploded poplar wood powder.
[0062] Example 4
[0063] This embodiment provides a method for preparing hydrogel by steam explosion pretreatment of all components of lignocellulose. Compared with Example 1, the amount of PVA solution in step (2) is controlled to be 50 parts by weight, and the rest is the same as Example 1.
[0064] Example 5
[0065] This embodiment provides a method for preparing hydrogel by steam explosion pretreatment of all components of lignocellulose. Compared with Example 1, the amount of PVA solution in step (2) is controlled to be 10 parts by weight, and the rest is the same as Example 1.
[0066] Example 6
[0067] This embodiment provides a method for preparing a hydrogel by steam explosion pretreatment of all components of lignocellulose. Compared with Example 1, the amount of steam-exploded corn stalks in step (2) is controlled to be 2 parts by mass, the amount of PVA solution is controlled to be 10 parts by mass, and the rest is the same as Example 1.
[0068] Comparative Example 1
[0069] This comparative example provides a method for preparing a hydrogel. Compared with Example 1, steam-exploded corn stalk powder is not added in step (2), and the rest is the same as Example 1.
[0070] Comparative Example 2
[0071] This comparative example provides a method for preparing a hydrogel using all components of lignocellulose. Compared with Example 1, an equal amount of steam-exploded corn stalk powder in step (2) is replaced by corn stalk powder, and the rest is the same as Example 1.
[0072] Comparative Example 3
[0073] This comparative example provides a method for preparing a hydrogel. Compared with comparative example 1, the concentration of the PVA solution in step (2) is controlled to be 20 wt %, and the rest is the same as comparative example 1.
[0074] Performance Characterization
[0075] The tensile properties of the hydrogels prepared in the examples and comparative examples were evaluated by the following method: a universal tensile testing machine was used to place the hydrogel precursor in a type 1 dumbbell sample mold and freeze-thaw to obtain a hydrogel sample, and the hydrogel sample was placed on a fixture for tensile testing to obtain a stress-strain curve of the hydrogel. The results are shown in FIG. Figure 1 , Figure 2 As shown in Table 1.
[0076] The hydrogels prepared in the examples and comparative examples were tested for their DPPH free radical (diphenyl-1-picryl radical) scavenging ability. The specific process was as follows: 10 mg of freeze-dried hydrogel powder was placed in 2 mL of methanol, mixed with 2 mL of DPPH-methanol solution (0.15 mmol / L), and reacted at room temperature in the dark for 30 minutes. The absorbance of the sample was measured at a wavelength of 517 nm using a UV-visible spectrophotometer P6. The DPPH free radical scavenging activity (RSA) of the sample was calculated according to the following formula:
[0077]
[0078] Here, A1 is the absorbance of the mixture containing the sample, A2 is the absorbance of the mixture containing no sample but 2 mL of methanol instead, and A3 is the absorbance of the mixture containing the sample and methanol.
[0079] The performance of the hydrogel prepared in the embodiment and the comparative example as a sand-fixing agent was tested. The specific method was as follows: the hydrogel sample was fully mixed with water of 9 times its mass, and the sample was crushed to prepare a test sample. The test sample was passed through the prepared hydrogel sand-fixing agent at 1.1 kg / m 2 The mixture was evenly sprayed on the surface of the sand dunes in a proportion of 200 μg / ml and dried at 50 °C for 12 h before testing. Wind erosion resistance test was carried out by simulating wind (10, 20 and 30 km / h). The weight of the sample was recorded every 5 min within 30 min and the weight loss rate was calculated.
[0080] Table 1
[0081]
[0082] “ / ” in the table means no data.
[0083] Table 2
[0084]
[0085] It can be seen from the data in the table that compared with Example 1, in Example 1, no steam-exploded corn stalks were added, and the fracture stress was significantly reduced. In Example 2, non-steam-exploded corn stalks were added, and its fracture stress was similar to that of Example 1, which was much lower than that of Example 1, indicating the key role of steam explosion in the formation of corn stalk hydrogel; Examples 4-6 used different ratios of steam-exploded corn stalks to PVA compared with Example 1. The ratios used in Examples 4-6 were 1:5, 1:1 and 2:1, respectively. Compared with Example 1, the ratio of steam-exploded corn stalks added in Example 5 was increased, but the mechanical properties of the hydrogel were significantly reduced. When the ratio of steam-exploded corn stalks to PVA was greater than 1:2, the mechanical properties could not be further improved, and Example 6 could not form a sample that could be used for detection, indicating that the ratio of steam-exploded corn stalks to PVA had better mechanical properties when it was 1:2-1:5.
[0086] The DPPH free radical scavenging rate was Figure 3As shown in Table 2, compared with Comparative Examples 1 and 2, the DPPH radical scavenging rate of Example 1 is significantly improved. This is because the steam explosion causes the lignin in the detonated corn stalks to be exposed, and the phenolic hydroxyl group with antioxidant activity (DPPH radical scavenging ability) acts on DPPH, thereby achieving the scavenging of DPPH radicals. The hydrogel of Comparative Example 1 does not contain lignin, and although the corn stalks in Comparative Example 2 contain lignin, the internal lignin cannot function because it has not been subjected to steam explosion treatment. This shows the important role of steam explosion pretreatment in improving the performance of corn stalk hydrogels.
[0087] The wind erosion rate results are as follows: Figure 4 As shown, compared with Comparative Example 3, the hydrogel prepared in Example 1 is superior to the hydrogel in Comparative Example 3 in preventing sand dunes from being eroded by wind, which proves the advantage of lignocellulose-based hydrogel in sand fixation.
[0088] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing hydrogel by steam explosion pretreatment of all components of lignocellulose, characterized in that: The method comprises the following steps: (1) subjecting the lignocellulose raw material to steam explosion treatment and then crushing the raw material to obtain a crushed lignocellulose raw material; (2) mixing the crushed lignocellulose raw material obtained in step (1) with the polyvinyl alcohol solution, and performing freeze-thaw treatment to obtain a lignocellulose full-component hydrogel; The mass ratio of the lignocellulose raw material to the polyvinyl alcohol in step (2) is 1-100%; The method does not perform modification treatment on the lignocellulose raw material and does not use a cross-linking agent and / or an initiator.
2. The method according to claim 1, characterized in that The lignocellulosic raw material is pre-impregnated before the steam explosion treatment in step (1); The water content of the pre-impregnated lignocellulose raw material is 30-66%.
3. The method according to claim 1, characterized in that The pressure of the steam explosion treatment in step (1) is 0.8-1.5 MPa.
4. The method according to claim 1, characterized in that: The pressure holding time of the steam explosion treatment in step (1) is 5-20 minutes.
5. The method according to claim 1, characterized in that The concentration of the polyvinyl alcohol solution in step (2) is 1-20wt%.
6. The method according to claim 1, characterized in that The alcoholysis degree of the polyvinyl alcohol in step (2) is in the range of 87% to 99%, and / or, The polyvinyl alcohol model includes any one of PVA1799, PVA1788 or PVA1750±50 or a combination of at least two of them.
7. The method according to claim 1, characterized in that In step (2), the mass ratio of the lignocellulose raw material to polyvinyl alcohol is 20-50%.
8. A lignocellulose full-component hydrogel, characterized in that: The lignocellulose full-component hydrogel is prepared by the method for preparing hydrogel by steam explosion pretreatment of lignocellulose full-components as described in any one of claims 1-7.
9. An application of the lignocellulose full-component hydrogel according to claim 8, characterized in that: The lignocellulose full-component hydrogel is used as a sand-fixing agent.
Citation Information
Patent Citations
Preparation method and application of all-component straw hydrogel
CN105504315A
Straw-based hydrogel adsorbent for efficiently removing heavy metal ions and preparation method thereof
CN110975832A
Method for increasing total-component utilization rate of agricultural straw raw materials
CN107557404A
Preparation method of high-cohesiveness antistatic fiber hydrogel
CN108841012A
Polyvinyl alcohol / lignin hydrogel with adjustable mechanical properties and preparation method thereof
CN115260530A