A glass fiber reinforced mobile phone back cover material and preparation method thereof
By combining modified glass fiber with polycarbonate resin and PMMA, the problem of insufficient rigidity of the back cover material of the mobile phone is solved, and glass fiber reinforced mobile phone back cover material with high strength and wear resistance is prepared to meet the needs of modern mobile phones. Dual performance requirements for lightweight and metal materials.
Patent Information
- Application Number
- CN202410409192.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-07
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-04-07
AI Technical Summary
The existing mobile phone back cover materials such as PMMA/PC composite boards are not rigid enough, which is difficult to meet consumers' requirements for portable electronic products. At the same time, the metal rear shell is eliminated at a faster speed, and new materials with metal strength and rigidity are needed.
Modified glass fiber is combined with polycarbonate resin and PMMA, and the glass fiber reinforced mobile phone is prepared by surface etching, epoxy silane coupling and 2,5-bis(aminomethyl)furan surface modification treatment. Cover material to improve the strength and wear resistance of the material.
The prepared glass fiber reinforced mobile phone back cover material has high strength, durability and scratch resistance, and has a good texture. It is suitable for the performance requirements of modern mobile phone materials, taking into account the rigidity of light and metal materials.
Abstract
Description
Technical Field
[0001] The invention relates to the field of mobile phone materials, and in particular to a glass fiber reinforced mobile phone back cover material and a preparation method thereof. Background Art
[0002] With the development of the times, smart phones are becoming more and more important in people's lives, and there are more and more types of mobile phones. The appearance of mobile phones is particularly important when purchasing. The material, craftsmanship and color of the mobile phone shell affect people's choices. Most of the current networks use large-scale MIMO technology, which requires adding a dedicated antenna to the mobile phone. Metal will shield and interfere with the signal, so the demetallization of the back cover of the mobile phone will be the general trend. At present, the material of the back cover of the mobile phone is shifting from metal to glass, ceramics and plastics, among which plastic is one of the most popular materials. However, ordinary injection molding + spraying back covers and protective covers cannot meet the requirements. The future trend is to get closer to metal or glass in terms of texture and experience.
[0003] As the elimination rate of metal mobile phone back shells further accelerates, glass / ceramic / plastic will become the three main raw materials. The raw material cost of PMMA / PC composite sheet is low and easy to process; 3D glass effect can be achieved through texture design and 3D high-pressure molding, and the visual texture of the surface is greatly enhanced; the back panel has good wear resistance and toughness. However, the current PMMA / PC composite board plastic mobile phone back cover has a low modulus and insufficient material rigidity, which makes it very easy to deform. With the development of technology and consumers' higher demand for portable electronic products, the requirements for lighter and thinner structural parts such as back covers are put forward. Therefore, the development of new materials with the strength and rigidity of metal materials and the decorative effect of plates has become a hot topic. Summary of the invention
[0004] In view of the problems existing in the prior art, the purpose of the present invention is to provide a glass fiber reinforced mobile phone back cover material and a preparation method thereof.
[0005] The purpose of the present invention is achieved by the following technical solutions:
[0006] In a first aspect, the present invention provides a method for preparing a glass fiber reinforced mobile phone back cover material, comprising the following steps:
[0007] Step 1, preparing modified glass fiber:
[0008] S1. Surface etching:
[0009] The glass fiber is subjected to a heating treatment in a sodium hydroxide solution, and after the treatment, the glass fiber is washed with water and dried to obtain an alkali-treated glass fiber;
[0010] S2, epoxy silane treatment:
[0011] The alkali-treated glass fiber is refluxed in an aqueous solution containing an epoxy silane coupling agent, and after the treatment, the alkali-treated glass fiber is washed with water and dried to obtain an epoxidized glass fiber;
[0012] S3. Surface modification:
[0013] The 2,5-di(aminomethyl)furan and epoxidized glass fiber are mixed in a solvent, subjected to a heating treatment, solids are filtered out, washed with alcohol at least three times, and vacuum dried to obtain modified glass fiber;
[0014] Step 2, preparing modified glass fiber-PC material:
[0015] The polycarbonate resin and the modified glass fiber are mixed in a mixing mixer, and after melting, they are mixed evenly to obtain a modified glass fiber-PC material;
[0016] Step 3, compound with PMMA:
[0017] Polymethyl methacrylate resin, modified glass fiber-PC material, compatibilizer and antioxidant are mixed in a screw extruder, and are sequentially melted, extruded and granulated to finally prepare a glass fiber reinforced mobile phone back cover material.
[0018] Preferably, the S1 process of step 1 specifically includes:
[0019] The glass fiber is mixed in a sodium hydroxide solution, heated to 40-50°C, and kept warm for 2-3 hours. After the treatment, the liquid is filtered out, washed with pure water until the washing liquid is neutral, and vacuum dried to obtain alkali-treated glass fiber.
[0020] More preferably, in the S1 process, the glass fiber has a length of 4-10 mm, a circular cross-section, a diameter of 10-15 μm, and a model of any one of E glass fiber, C glass fiber, and E-CR glass fiber.
[0021] More preferably, in the S1 process, the concentration of the sodium hydroxide solution is 1-3 mol / L, and the mass ratio of the glass fiber to the sodium hydroxide solution is 1:10-20.
[0022] Preferably, the S2 process of step 1 specifically includes:
[0023] Take the coupling agent KH-560 and dissolve it in deionized water, then add the alkali-treated glass fiber, heat it to 50-80°C, stir it for 4-8h, after the treatment, filter out the liquid, wash it with water for at least three times, and vacuum dry it to obtain the epoxidized glass fiber.
[0024] More preferably, in the S2 process, the epoxy silane coupling agent is coupling agent KH-560, and the mass ratio of the alkali-treated glass fiber, coupling agent KH-560 and deionized water is 1:0.12-0.24:10-20.
[0025] Preferably, the S3 process of step 1 specifically includes:
[0026] Take 2,5-di(aminomethyl)furan and dissolve it in N,N-dimethylformamide, add epoxidized glass fiber, heat to 50-60°C, and keep warm for 5-15 hours. After the treatment, filter out the solid, wash with alcohol for at least three times, and vacuum dry to obtain modified glass fiber.
[0027] More preferably, in the S3 process, the mass ratio of epoxidized glass fiber, 2,5-bis(aminomethyl)furan and N,N-dimethylformamide is 1:0.37-0.55:8-16.
[0028] Preferably, in step 2, the density of the polycarbonate resin is 1.19-1.21 g / cm 3 , the melt index is 8±0.3g / 10min (300℃, 1.2kg).
[0029] Preferably, in step 2, the mass ratio of the polycarbonate resin to the modified glass fiber is 100:20-40.
[0030] Preferably, in step 2, the melting temperature is 220-280° C., and the mixing time is 3-8 min.
[0031] Preferably, in step 3, the mass ratio of polymethyl methacrylate resin, modified glass fiber-PC material, compatibilizer and antioxidant is 18-30:45-65:2.6-4.8:0.5-1.
[0032] Preferably, in step 3, the density of the polymethyl methacrylate resin is 1.18-1.19 g / cm 3 , the melt index is 3.4±0.2g / 10min (230℃, 3.8kg).
[0033] Preferably, in step 3, the compatibilizer is a styrene / acrylonitrile / maleic anhydride copolymer, model SMA-700, with a maleic anhydride content of 18% and a melt index of 5±0.5 g / 10 min (190° C., 2.16 kg).
[0034] Preferably, in step 3, the antioxidant is a hindered phenol antioxidant, and the model is BASF antioxidant Irganox 245 or BASF antioxidant Irganox 1076.
[0035] Preferably, in step 3, the rotation speed of the screw extruder is 300-500 r / min, the aspect ratio (L / D) of the screw is 50-60, and the temperature range is 235-295°C.
[0036] In a second aspect, the present invention provides a glass fiber reinforced mobile phone back cover material, which is prepared by the above-mentioned preparation method.
[0037] The beneficial effects of the present invention are:
[0038] 1. The present invention prepares a mobile phone back cover material, which is a modified glass fiber reinforced material. The material can make the thickness of the composite board reach 0.5 mm or less. On the basis of being lighter and thinner, it can also have good metal material strength and rigidity, good texture, good hand feel, and is not easy to scratch. It can basically meet the performance requirements of most mobile phone material manufacturers for back cover materials.
[0039] 2. Different from the traditional glass fiber reinforced PMMA / PC composite material, the modified glass fiber reinforced material prepared by the present invention has undergone a series of modifications to the glass fiber, and then compounded with PC material and PMMA material in turn. The prepared material has high strength and high wear resistance even if it is thin, and has good durability and scratch resistance.
[0040] 3. The modified glass fiber reinforced material prepared by the present invention comprises the following steps: firstly, the glass fiber is subjected to alkaline light etching treatment, the purpose of which is to enhance the active groups on the surface of the glass fiber; then, the surface of the glass fiber is treated with an epoxy silane coupling agent, so that the surface of the glass fiber is rich in a large number of epoxy groups; and then, 2,5-bis(aminomethyl)furan is used to perform surface modification treatment on the epoxidized glass fiber. 2,5-bis(aminomethyl)furan contains diamino groups and furan groups, wherein the amino groups can be combined with the epoxy groups on the glass fiber, so that a large number of furan groups are fixed on the surface of the glass fiber, thereby enhancing the performance of the glass fiber surface; on the other hand, the reaction product of the epoxy group and the amino group also enhances the surface activity of the glass fiber, and the interface bonding performance with the PC resin is also well improved, thereby finally improving the comprehensive performance of the composite material. DETAILED DESCRIPTION
[0041] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0042] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0043] In the examples and comparative examples of the present invention, some of the raw materials used are as follows:
[0044] The density of polycarbonate resin is 1.19-1.21g / cm 3 , the melt index is 8±0.3g / 10min (300℃, 1.2kg).
[0045] The density of polymethyl methacrylate resin is 1.18-1.19g / cm 3 , the melt index is 3.4±0.2g / 10min (230℃, 3.8kg).
[0046] The glass fiber has a length of 4-10 mm, a circular cross section, and a diameter of 10-15 μm.
[0047] The compatibilizer is a styrene / acrylonitrile / maleic anhydride copolymer, model SMA-700, maleic anhydride content is 18%, and melt index is 5±0.5g / 10min (190°C, 2.16kg).
[0048] The present invention will be further described below in conjunction with the following examples.
[0049] Example 1
[0050] A glass fiber reinforced mobile phone back cover material, the preparation method comprises the following steps:
[0051] Step 1, preparing modified glass fiber:
[0052] S1. Surface etching:
[0053] The C glass fiber is mixed with a 2 mol / L sodium hydroxide solution, the mass ratio of the glass fiber to the sodium hydroxide solution is 1:15, the temperature is raised to 45°C, and the heat treatment is carried out for 2 hours. After the treatment, the liquid is filtered out, and the washing liquid is washed with pure water until the washing liquid is neutral, and vacuum dried to obtain an alkali-treated glass fiber;
[0054] S2, epoxy silane treatment:
[0055] Coupling agent KH-560 was dissolved in deionized water, and then alkali-treated glass fiber was added. The mass ratio of alkali-treated glass fiber, coupling agent KH-560 and deionized water was 1:0.18:15. The temperature was raised to 60°C and stirred for 6 hours. After the treatment, the liquid was filtered out, washed with water for at least three times, and vacuum dried to obtain epoxidized glass fiber.
[0056] S3. Surface modification:
[0057] Take 2,5-bis(aminomethyl)furan and dissolve it in N,N-dimethylformamide, add epoxidized glass fiber, the mass ratio of epoxidized glass fiber, 2,5-bis(aminomethyl)furan and N,N-dimethylformamide is 1:0.46:12, heat to 55°C, keep warm for 10 hours, after the treatment, filter out the solid, wash with alcohol for at least three times, and vacuum dry to obtain modified glass fiber.
[0058] Step 2, preparing modified glass fiber-PC material:
[0059] The polycarbonate resin and the modified glass fiber are mixed in a mixing mixer, the mass ratio of the polycarbonate resin and the modified glass fiber is 100:30, and the mixture is evenly mixed after melting, the melting temperature is 250° C., and the mixing time is 5 minutes, to obtain a modified glass fiber-PC material;
[0060] Step 3, compound with PMMA:
[0061] Polymethyl methacrylate resin, modified glass fiber-PC material, compatibilizer SMA-700 and BASF antioxidant Irganox1076 are mixed in a screw extruder, the mass ratio of polymethyl methacrylate resin, modified glass fiber-PC material, compatibilizer and antioxidant is 24:55:3.7:0.6, and they are melted, extruded and granulated in sequence. The speed of the screw extruder is 400 r / min, the aspect ratio (L / D) of the screw is 55, and the temperature range is 235-295°C. Finally, a glass fiber reinforced mobile phone back cover material is prepared.
[0062] Example 2
[0063] A glass fiber reinforced mobile phone back cover material, the preparation method comprises the following steps:
[0064] Step 1, preparing modified glass fiber:
[0065] S1. Surface etching:
[0066] The E glass fiber was mixed with a 1 mol / L sodium hydroxide solution, the mass ratio of the glass fiber to the sodium hydroxide solution was 1:10, the temperature was raised to 40°C, and the heat treatment was carried out for 3 hours. After the treatment, the liquid was filtered out, and the glass fiber was washed with pure water until the washing liquid was neutral, and vacuum dried to obtain an alkali-treated glass fiber.
[0067] S2, epoxy silane treatment:
[0068] Dissolve the coupling agent KH-560 in deionized water, then add alkali-treated glass fiber, the mass ratio of alkali-treated glass fiber, coupling agent KH-560 and deionized water is 1:0.12:10, heat to 50°C, stir for 8 hours, filter to remove the liquid after the treatment, wash with water for at least three times, and vacuum dry to obtain epoxidized glass fiber;
[0069] S3. Surface modification:
[0070] Take 2,5-bis(aminomethyl)furan and dissolve it in N,N-dimethylformamide, add epoxidized glass fiber, the mass ratio of epoxidized glass fiber, 2,5-bis(aminomethyl)furan and N,N-dimethylformamide is 1:0.37:8, heat to 50°C, keep warm for 5 hours, after the treatment, filter out the solid, wash with alcohol for at least three times, and vacuum dry to obtain modified glass fiber.
[0071] Step 2, preparing modified glass fiber-PC material:
[0072] The polycarbonate resin and the modified glass fiber are mixed in a mixing mixer, the mass ratio of the polycarbonate resin and the modified glass fiber is 100:20, and the mixture is evenly mixed after melting, the melting temperature is 220° C., and the mixing time is 8 minutes, to obtain a modified glass fiber-PC material;
[0073] Step 3, compound with PMMA:
[0074] Polymethyl methacrylate resin, modified glass fiber-PC material, compatibilizer SMA-700 and BASF antioxidant Irganox245 are mixed in a screw extruder, the mass ratio of polymethyl methacrylate resin, modified glass fiber-PC material, compatibilizer and antioxidant is 18:45:2.6:0.5, and they are melted, extruded and granulated in sequence. The speed of the screw extruder is 300 r / min, the aspect ratio (L / D) of the screw is 55, and the temperature range is 235-295°C. Finally, a glass fiber reinforced mobile phone back cover material is prepared.
[0075] Example 3
[0076] A glass fiber reinforced mobile phone back cover material, the preparation method comprises the following steps:
[0077] Step 1, preparing modified glass fiber:
[0078] S1. Surface etching:
[0079] The E-CR glass fiber was mixed with a 3 mol / L sodium hydroxide solution, the mass ratio of the glass fiber to the sodium hydroxide solution was 1:20, the temperature was raised to 50°C, and the heat treatment was carried out for 2 hours. After the treatment, the liquid was filtered out, and the glass fiber was washed with pure water until the washing liquid was neutral, and vacuum dried to obtain an alkali-treated glass fiber.
[0080] S2, epoxy silane treatment:
[0081] Coupling agent KH-560 was dissolved in deionized water, and then alkali-treated glass fiber was added. The mass ratio of alkali-treated glass fiber, coupling agent KH-560 and deionized water was 1:0.24:20. The temperature was raised to 80°C and stirred for 4 hours. After the treatment, the liquid was filtered out, washed with water for at least three times, and vacuum dried to obtain epoxidized glass fiber.
[0082] S3. Surface modification:
[0083] Take 2,5-bis(aminomethyl)furan and dissolve it in N,N-dimethylformamide, add epoxidized glass fiber, the mass ratio of epoxidized glass fiber, 2,5-bis(aminomethyl)furan and N,N-dimethylformamide is 1:0.55:16, heat to 60°C, keep warm for 5 hours, after the treatment, filter out the solid, wash with alcohol for at least three times, and vacuum dry to obtain modified glass fiber.
[0084] Step 2, preparing modified glass fiber-PC material:
[0085] The polycarbonate resin and the modified glass fiber are mixed in a mixing mixer, the mass ratio of the polycarbonate resin and the modified glass fiber is 100:40, and the mixture is evenly mixed after melting, the melting temperature is 280° C., and the mixing time is 3 minutes, to obtain a modified glass fiber-PC material;
[0086] Step 3, compound with PMMA:
[0087] Polymethyl methacrylate resin, modified glass fiber-PC material, compatibilizer SMA-700 and BASF antioxidant Irganox245 are mixed in a screw extruder, the mass ratio of polymethyl methacrylate resin, modified glass fiber-PC material, compatibilizer and antioxidant is 30:65:4.8:1, and they are melted, extruded and granulated in sequence. The speed of the screw extruder is 500 r / min, the aspect ratio (L / D) of the screw is 55, and the temperature range is 235-295°C. Finally, a glass fiber reinforced mobile phone back cover material is prepared.
[0088] Comparative Example 1
[0089] A glass fiber reinforced mobile phone back cover material, the preparation method is different from that of Example 1 in that: the glass fiber in step 1 is not modified, the modified glass fiber in step 2 is replaced by ordinary glass fiber, the polycarbonate resin and the ordinary glass fiber are compounded in step 2 to obtain a modified glass fiber-PC material, and the mass ratio of the polycarbonate resin to the glass fiber is 100:30. The other components and the preparation method remain unchanged.
[0090] Comparative Example 2
[0091] A glass fiber reinforced mobile phone back cover material, the preparation method is different from that of Example 1 in that: the modified glass fiber in step 1 is replaced with epoxidized glass fiber (prepared by referring to S1 and S2 of Example 1), and in step 2, polycarbonate resin and epoxidized glass fiber are compounded to obtain a modified glass fiber-PC material, and the mass ratio of polycarbonate resin to epoxidized glass fiber is 100:30. The other components and the preparation method remain unchanged.
[0092] Comparative Example 3
[0093] A glass fiber reinforced mobile phone back cover material, the preparation method is different from that of Example 1 in that: in step 1, the modified glass fiber is replaced by epoxidized glass fiber (prepared by referring to S1 and S2 of Example 1); in step 2, polycarbonate resin, 2,5-di(aminomethyl)furan, and epoxidized glass fiber are compounded to obtain a modified glass fiber-PC material, and the mass ratio of polycarbonate resin, 2,5-di(aminomethyl)furan, and epoxidized glass fiber is 100:10.65:19.35. The remaining components and the preparation method remain unchanged.
[0094] In order to further demonstrate the content of the present invention, the performance of the mobile phone back cover materials prepared in Example 1 of the present invention and Comparative Examples 1-3 were tested respectively, and the test contents included: tensile strength (reference standard ASTM D638), flexural strength (reference standard ASTM D790), cantilever beam notched impact strength (reference standard ASTM D256), hardness (reference standard ASTMD3363), and the test results are summarized in Table 1 below.
[0095] Table 1 Test results of the performance of different mobile phone back cover materials
[0096] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Tensile strength(MPa) 86.3 67.6 73.5 71.7 Bending strength(MPa) 117.9 97.2 105.2 102.6 Notched impact strength (J / m) 792.6 695.3 731.0 712.8 Hardness (pencil) 3H H 2H 2H
[0097] From the test results in Table 1, it can be seen that the glass fiber reinforced mobile phone back cover material prepared in Example 1 can take into account the performance of strength, hardness and toughness. Due to the poor compatibility of glass fiber and polycarbonate in Comparative Example 1, the performance of the back cover material prepared subsequently is insufficient in all aspects; the performance of Comparative Example 3 is slightly weaker than that of Comparative Example 2. The possible reason is that after the amount of glass fiber is reduced, the performance of 2,5-di(aminomethyl)furan alone cannot fully make up for that part of strength and toughness, so its performance lags behind that of Comparative Example 2.
[0098] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0099] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a glass fiber reinforced mobile phone back cover material, characterized in that: The following steps are involved: Step 1, preparing modified glass fiber: S1. Surface etching: The glass fiber is subjected to a heating treatment in a sodium hydroxide solution, and after the treatment, the glass fiber is washed with water and dried to obtain an alkali-treated glass fiber; S2, epoxy silane treatment: The alkali-treated glass fiber is refluxed in an aqueous solution containing an epoxy silane coupling agent, and after the treatment, the alkali-treated glass fiber is washed with water and dried to obtain an epoxidized glass fiber; S3. Surface modification: The 2,5-di(aminomethyl)furan and epoxidized glass fiber are mixed in a solvent, subjected to a heating treatment, solids are filtered out, washed with alcohol at least three times, and vacuum dried to obtain modified glass fiber; Step 2, preparing modified glass fiber-PC material: The polycarbonate resin and the modified glass fiber are mixed in a mixing mixer, and after melting, they are mixed evenly to obtain a modified glass fiber-PC material; Step 3, compound with PMMA: Polymethyl methacrylate resin, modified glass fiber-PC material, compatibilizer and antioxidant are mixed in a screw extruder, and melted, extruded and granulated in sequence to finally prepare a glass fiber reinforced mobile phone back cover material; The S3 process of step 1 specifically includes: Dissolve 2,5-di(aminomethyl)furan in N,N-dimethylformamide, add epoxidized glass fiber, heat to 50-60°C, and keep warm for 5-15 hours. After the treatment, filter out the solid, wash with alcohol at least three times, and vacuum dry to obtain modified glass fiber; In S3, the mass ratio of epoxidized glass fiber, 2,5-di(aminomethyl)furan and N,N-dimethylformamide is 1:0.37-0.55:8-16; In the step 2, the mass ratio of the polycarbonate resin to the modified glass fiber is 100:20-40; In the step 3, the mass ratio of polymethyl methacrylate resin, modified glass fiber-PC material, compatibilizer and antioxidant is 18-30:45-65:2.6-4.8:0.5-1.
2. The method for preparing a glass fiber reinforced mobile phone back cover material according to claim 1, characterized in that: The S1 process of step 1 specifically includes: The glass fiber is mixed with a sodium hydroxide solution, heated to 40-50°C, and kept warm for 2-3 hours. After the treatment, the liquid is filtered out, washed with pure water until the washing liquid is neutral, and vacuum dried to obtain an alkali-treated glass fiber; The concentration of the sodium hydroxide solution is 1-3 mol / L, and the mass ratio of the glass fiber to the sodium hydroxide solution is 1:10-20.
3. The method for preparing a glass fiber reinforced mobile phone back cover material according to claim 1, characterized in that: The S2 process of step 1 specifically includes: Dissolve the coupling agent KH-560 in deionized water, then add alkali-treated glass fiber, heat to 50-80°C, stir for 4-8h, filter to remove the liquid after the treatment, wash with water at least three times, and vacuum dry to obtain epoxidized glass fiber; The epoxy silane coupling agent is coupling agent KH-560, and the mass ratio of alkali-treated glass fiber, coupling agent KH-560 and deionized water is 1:0.12-0.24:10-20.
4. The method for preparing a glass fiber reinforced mobile phone back cover material according to claim 1, characterized in that: In step 2, the density of the polycarbonate resin is 1.19-1.21 g / cm 3 The melt index is 8±0.3g / 10min at 300℃ and 1.2kg.
5. The method for preparing a glass fiber reinforced mobile phone back cover material according to claim 1, characterized in that: In the step 2, the melting temperature is 220-280° C., and the mixing time is 3-8 min.
6. The method for preparing a glass fiber reinforced mobile phone back cover material according to claim 1, characterized in that: In step 3, the density of the polymethyl methacrylate resin is 1.18-1.19 g / cm 3 The melt index is 3.4±0.2g / 10min at 230℃ and 3.8kg. The compatibilizer is styrene / acrylonitrile / maleic anhydride copolymer, model SMA-700, maleic anhydride content is 18%, and the melt index is 5±0.5g / 10min at 190℃ and 2.16kg.
7. The method for preparing a glass fiber reinforced mobile phone back cover material according to claim 1, characterized in that: In the step 3, the antioxidant is a hindered phenol antioxidant, and the model is BASF antioxidant Irganox 245 or BASF antioxidant Irganox 1076.
8. A glass fiber reinforced mobile phone back cover material, characterized in that: The preparation method according to claim 1 is used for preparation.
Citation Information
Patent Citations
Use of 2,5-bis(aminomethyl)furan as a hardener for epoxy resins
CN105452323A
Glass fiber reinforced PMMA composite material and preparation method thereof
CN113234296A
Glass fiber for glass paper
JP1995291675A
Glass fiber reinforced polycarbonate material, and preparation method and application thereof
WO2024027415A1