A method for preparing a back contact heterojunction solar cell
Through laser grooving and inkjet masking combined with wet etching process, the preparation process of back-junction back-contact heterojunction solar cells is simplified, solving the complex process and mass production problems in the existing technology, and improving the cell conversion efficiency. and equipment service life.
Patent Information
- Application Number
- CN202410293032.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-03-14
AI Technical Summary
The preparation process of existing back-junction back-contact heterojunction solar cells is complex, the production line length is long, equipment and material requirements are high, and the preparation yield is low, making it difficult to achieve mass production.
Using laser grooving and inkjet masking combined with wet etching process, unnecessary film layers are removed by depositing multi-layer films and inkjet printing alkali corrosion resistant wet film materials to form an interdigitated structure, simplifying the process and Reduce risk of injury.
Efficient and simple preparation of back-junction back-contact heterojunction solar cells has been achieved, which improves conversion efficiency, reduces equipment damage and process complexity, and advances the possibility of mass production.
Smart Images

Figure CN118173662B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of heterojunction solar cells, in particular to a method for preparing a back-contact heterojunction solar cell. Background Art
[0002] Back-junction back-contact heterojunction solar cells are considered to be the most efficient structure of crystalline silicon single-junction solar cells because there is no metal grid line blocking the front and amorphous silicon thin film is introduced on the back for efficient surface passivation. However, despite its potential for ultra-high conversion efficiency, since both the positive and negative electrodes are on the back, the need to prepare the positive and negative electrodes with interdigitated spacing has become a difficulty in the preparation process, and there is no unified solution yet. At present, some people have proposed to prepare back-junction back-contact heterojunction solar cells by multiple mask exposure and development, and a conversion efficiency of 26.7% has been achieved in the laboratory, but the mask exposure technology is complex, the production line length is too long and the process is cumbersome, it has very high requirements for equipment and materials, and the preparation yield is low, so it cannot become a mass production process. Summary of the invention
[0003] The purpose of the present invention is to improve and innovate the shortcomings and problems existing in the background technology and provide a method for preparing a back-contact heterojunction solar cell.
[0004] A method for preparing a back-contact heterojunction solar cell comprises the following steps:
[0005] Pre-treating the silicon wafer surface;
[0006] Depositing a first intrinsic amorphous silicon thin film layer, a first phosphorus-doped silicon-based thin film layer, a silicon nitride thin film layer, and a second intrinsic amorphous silicon thin film layer in sequence on the front side of the silicon wafer;
[0007] Depositing a third intrinsic amorphous silicon thin film layer and a boron-doped silicon-based thin film layer in sequence on the back side of the silicon wafer;
[0008] The back side of the silicon wafer is grooved by laser, wherein the groove depth is greater than the thickness of the boron-doped silicon-based thin film layer, but less than the sum of the thickness of the third intrinsic amorphous silicon thin film layer and the boron-doped silicon-based thin film layer;
[0009] Depositing a fourth intrinsic amorphous silicon thin film layer and a second phosphorus-doped silicon-based thin film layer on the back side of the silicon wafer;
[0010] A layer of anti-alkali corrosion wet film material is applied on the laser slotted area by inkjet printing or screen printing. The width of the wet film material is 2um-20um greater than the laser slotted width.
[0011] The silicon wafer is cleaned with an alkaline solution to remove the second intrinsic amorphous silicon thin film layer on the front side of the silicon wafer and the second phosphorus-doped silicon-based thin film layer and the fourth intrinsic amorphous silicon thin film layer on the back side of the silicon wafer that are not protected by the wet film material; the silicon wafer is cleaned with an acid solution to remove the silicon nitride thin film layer on the front side of the silicon wafer and the wet film material on the back side of the silicon wafer;
[0012] Depositing a transparent conductive film layer on the back of the silicon wafer;
[0013] Using laser to isolate and scribe the transparent conductive film layer to block the lateral conduction between the second phosphorus-doped silicon-based film layer and the boron-doped silicon-based film layer;
[0014] A metal electrode is prepared on the back of the silicon wafer. The metal electrode corresponding to the second phosphorus-doped silicon-based thin film layer is the negative electrode of the solar cell, and the metal electrode corresponding to the boron-doped silicon-based thin film layer is the positive electrode of the solar cell.
[0015] A further solution is that the step of cleaning the silicon wafer with an acid solution to remove the silicon nitride film layer on the front side of the silicon wafer and the wet film material on the back side of the silicon wafer comprises:
[0016] A thin film interference layer is deposited on the front side of the silicon wafer, wherein the thin film interference layer includes but is not limited to one or more stacked thin films selected from the group consisting of a silicon nitride thin film layer, a silicon oxynitride thin film layer, and a silicon oxide thin film layer, the thickness of the thin film interference layer is between 60nm and 200nm, the refractive index of the thin film is between 1.4 and 3.0, and the refractive index of the thin film interference layer increases from top to bottom.
[0017] A further solution is that the step of using a laser to groove the back of the silicon wafer, wherein the groove depth is greater than the thickness of the boron-doped silicon-based thin film layer and less than the sum of the thicknesses of the third intrinsic amorphous silicon thin film layer and the boron-doped silicon-based thin film layer, comprises:
[0018] The silicon wafer surface is cleaned to remove contaminants and oxides generated during the laser ablation process.
[0019] A further solution is that the step of cleaning the surface of the silicon wafer to remove pollutants and oxides generated during the laser ablation process specifically includes:
[0020] The silicon wafer is transferred to a wet process device for cleaning, and the surface of the silicon wafer is cleaned with a hydrofluoric acid aqueous solution to remove pollutants and oxides on the surface of the silicon wafer.
[0021] A further solution is that the phosphorus-doped silicon-based thin film layer can be a phosphorus-doped amorphous silicon thin film layer, a phosphorus-doped microcrystalline silicon thin film layer, or a phosphorus-doped microcrystalline silicon oxide thin film; the boron-doped silicon-based thin film layer can be a boron-doped amorphous silicon thin film layer, a boron-doped microcrystalline silicon thin film layer, or a boron-doped microcrystalline silicon oxide thin film.
[0022] A further solution is that the step of pre-treating the surface of the silicon wafer includes:
[0023] First, the double-sided silicon wafer is textured, and then the organic pollutants and metal ion pollutants on the surface of the silicon wafer are removed using acidic and alkaline solutions. Finally, the silicon wafer is immersed in a hydrofluoric acid aqueous solution to remove the oxide layer on the surface of the silicon wafer and is dried.
[0024] A further solution is that the wavelength of the laser used to groove the back of the silicon wafer is between 200nm-500nm, the laser is a nanosecond laser, a femtosecond laser or a picosecond laser, the frequency is 10E12HZ-10E19HZ, the laser groove width is 10um-100um, and the interval between adjacent laser grooves is 30-300um.
[0025] A further solution is that the step of coating a layer of alkali corrosion resistant wet film material on the laser slotted area, wherein the width of the wet film material is 2um-20um greater than the laser slotted width, specifically comprises:
[0026] A layer of alkali corrosion-resistant wet film material is coated on the laser slotted area by inkjet printing or screen printing, and the width of the wet film material is 30-120um.
[0027] A further solution is that the step of depositing a transparent conductive film layer on the back side of the silicon wafer specifically includes:
[0028] A transparent conductive film layer is deposited on the back of the silicon wafer by magnetron sputtering or reactive plasma deposition. The transparent conductive film layer can be an indium-containing conductive oxide or an indium-free conductive oxide. The thickness of the transparent conductive film layer is 30nm-300nm, and the refractive index of the film is between 1.7-3.0.
[0029] A further solution is that the wavelength of the laser used to isolate and scribe the transparent conductive film layer is between 200nm and 500nm, the laser type is one of nanosecond laser, femtosecond laser or picosecond laser, the frequency is 10E12HZ-10E19HZ, and the width of the laser scribe is 1um-50um.
[0030] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention proposes a relatively low-cost and relatively simple process technology route, which firstly utilizes the convenience of laser ablation to prepare patterns, and also adopts the inkjet mask method to replace the one-step laser ablation method to avoid the disadvantages of multiple laser etching damaging the intrinsic amorphous silicon layer to reduce the passivation effect, and finally introduces an efficient and simple process technology route, which is expected to promote the large-scale mass production of high-efficiency back-junction back-contact heterojunction solar cells. Specifically, the present invention coats a layer of alkali corrosion-resistant wet film material on the laser grooved area by the inkjet mask method, and then removes the second phosphorus-doped silicon-based thin film layer and the fourth intrinsic amorphous silicon thin film layer on the back that are not protected by the wet film material by an alkaline solution, and then removes the wet film material by an acid solution to obtain a cross-finger structure of a boron-doped silicon-based thin film and a phosphorus-doped silicon-based thin film arranged at intervals. The present invention adopts alkali-resistant wet film protection combined with wet etching process. Compared with directly laser ablating the second phosphorus-doped silicon-based thin film layer and the fourth intrinsic amorphous silicon thin film layer, the damage to the boron-doped silicon-based thin film layer is reduced, and the risk of intrinsic amorphous silicon passivation failure caused by laser ablation is avoided, thereby reducing damage to the silicon wafer and improving the conversion efficiency of the battery. Compared with the three-step laser ablation method, one laser process is also reduced. The application of the technology of the present invention can more efficiently mass-produce back-junction back-contact heterojunction solar cells; in addition, the present application improves the interface passivation effect and field passivation effect of the laser groove area by depositing the fourth intrinsic amorphous silicon thin film layer and the second phosphorus-doped silicon-based thin film layer, respectively, and improves the conversion efficiency of the battery. Moreover, the present application adopts the inkjet mask method to coat a layer of alkali-resistant wet film material on the laser groove area to obtain a forked finger structure of spaced boron-doped silicon-based thin films and phosphorus-doped silicon-based thin films, and will not damage the passivation effect of the intrinsic amorphous silicon thin film layer in the laser groove area. More importantly, the present application deposits a first intrinsic amorphous silicon thin film layer, a first phosphorus-doped silicon-based thin film layer, a silicon nitride thin film layer and a second intrinsic amorphous silicon thin film layer in sequence on the front side of the silicon wafer; the second intrinsic amorphous silicon thin film layer is used to prevent the front side of the silicon wafer from being corroded by an acid solution, so that a hydrofluoric acid aqueous solution can be used to clean the contaminants and oxides in the laser grooved area, and the silicon nitride thin film layer on the front side of the silicon wafer prevents the front side of the silicon wafer from being corroded by an alkaline solution, so that a layer of alkali-corrosion-resistant wet film material can be coated on the laser grooved area accordingly, thereby avoiding the disadvantage of multiple laser etching causing damage to the intrinsic amorphous silicon layer to reduce the passivation effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0032] Figure 1It is a schematic diagram of the method flow of the present invention;
[0033] Figure 2 This is a schematic diagram of the silicon wafer structure with four layers of thin films deposited on the front side of the present invention;
[0034] Figure 3 This is a schematic diagram of the structure of a silicon wafer with two layers of thin films deposited on the back of the present invention;
[0035] Figure 4 This is a schematic diagram of the structure of a silicon wafer with laser grooves on the back side of the present invention;
[0036] Figure 5 This is a schematic diagram of the structure of a silicon wafer with a wet film material coated on the back of the present invention;
[0037] Figure 6 This is a schematic diagram of the silicon wafer structure for removing the wet film material and the silicon nitride film layer according to the present invention;
[0038] Figure 7 This is a schematic diagram of the silicon wafer structure with a thin film interference layer deposited on the front side of the present invention;
[0039] Figure 8 This is a schematic diagram of the silicon wafer structure with a transparent conductive film layer deposited on the back of the present invention;
[0040] Fig. 9 This is a schematic diagram of the structure of a silicon wafer with back laser scribing according to the present invention;
[0041] Fig.10 It is a schematic diagram of the structure of a back-contact heterojunction solar cell of the present invention;
[0042] Figure numerals: metal electrode 1, first intrinsic amorphous silicon thin film layer 2, first phosphorus-doped silicon-based thin film layer 3, silicon nitride thin film layer 4, second intrinsic amorphous silicon thin film layer 5, third intrinsic amorphous silicon thin film layer 6, boron-doped silicon-based thin film layer 7, fourth intrinsic amorphous silicon thin film layer 8, second phosphorus-doped silicon-based thin film layer 9, wet film material 10, thin film interference layer 11, transparent conductive thin film layer 12. DETAILED DESCRIPTION
[0043] In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0044] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.
[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0046] Step S1, pre-treating the surface of the silicon wafer;
[0047] Specifically, a conventional alkaline texturing process is used to make a pyramid structure on the front and back sides of the silicon wafer to reduce the reflectivity of the silicon wafer surface; at the same time, the texturized silicon wafer is cleaned with different acidic solutions and alkaline solutions to remove organic pollutants and metal ion pollutants on the surface of the silicon wafer. Finally, the silicon wafer is immersed in a hydrofluoric acid aqueous solution to remove the oxide layer on the surface of the silicon wafer and dried to obtain a double-sided texturized silicon wafer structure with a clean surface.
[0048] It should be noted that the silicon wafer of the present application is an N-type silicon wafer.
[0049] Step S2, depositing a first intrinsic amorphous silicon thin film layer, a first phosphorus-doped silicon-based thin film layer, a silicon nitride thin film layer, and a second intrinsic amorphous silicon thin film layer in sequence on the front side of the silicon wafer;
[0050] A first intrinsic amorphous silicon thin film layer 2, a first phosphorus-doped silicon-based thin film layer 3, a silicon nitride thin film layer 4, and a second intrinsic amorphous silicon thin film layer 5 are sequentially deposited on the front surface of the silicon wafer by chemical vapor deposition, a total of four thin films, such as Figure 2 shown.
[0051] Wherein: the purpose of depositing the first intrinsic amorphous silicon thin film layer 2 is to passivate the dangling bonds on the silicon wafer surface and reduce the surface defect state density; the thickness of this film layer is 4n-10nm, and the refractive index is between 3.5-4.4.
[0052] The purpose of depositing the first phosphorus-doped silicon-based thin film layer 3 is to further provide a field passivation effect for the surface and improve the battery conversion efficiency; the thickness of this film layer is 4n-30nm, and the refractive index is between 2.2-4.5.
[0053] It should be noted that the first phosphorus-doped silicon-based thin film layer 3 may be an amorphous silicon thin film or a microcrystalline silicon thin film or a microcrystalline silicon oxide thin film, and this application does not make any specific limitation thereto, and all of them are within the protection scope of this application.
[0054] The purpose of the deposited silicon nitride film layer 4 is to protect the underlying amorphous silicon layer from subsequent etching by the alkaline solution. This film layer can also be silicon oxide, silicon oxynitride and other films. This application does not make specific limitations and all are within the protection scope of this application. The thickness of this film layer is 10nm-200nm, and the refractive index is between 1.4-4.5.
[0055] The purpose of depositing the second intrinsic amorphous silicon film layer 5 is to protect the silicon nitride film layer 4 from being etched by an acidic solution. This film layer can be intrinsic amorphous silicon or phosphorus-doped or carbon-doped amorphous silicon or microcrystalline silicon film. This application does not make specific limitations and all are within the protection scope of this application. This film layer has a thickness of 10nm-100nm and a refractive index between 2.2-4.5.
[0056] Step S3, depositing a third intrinsic amorphous silicon thin film layer 6 and a boron-doped silicon-based thin film layer 7 on the back side of the silicon wafer in sequence;
[0057] A third intrinsic amorphous silicon thin film layer 6 and a boron-doped silicon-based thin film layer 7 are sequentially deposited on the back of the silicon wafer by chemical vapor deposition. Figure 3 As shown;
[0058] Among them: the third intrinsic amorphous silicon film layer 6 is used to passivate the dangling bonds on the silicon wafer surface and reduce the surface defect state density; the film thickness of this layer is 4n-10nm, and the refractive index is between 3.5-4.4.
[0059] The boron-doped silicon-based thin film layer 7 can be a boron-doped amorphous silicon thin film, a boron-doped microcrystalline silicon thin film, or a boron-doped microcrystalline silicon oxide thin film, and the boron-doped silicon-based thin film layer 7 is a P-type boron-doped silicon-based thin film layer, the purpose of which is to form a PN junction with the N-type silicon wafer deposited in the present application to improve the battery conversion efficiency; the thickness of this film layer is 10nm-50nm, and the refractive index is between 2.2-4.5.
[0060] Step S4, using laser to groove the back of the silicon wafer, wherein the groove depth is greater than the thickness of the boron-doped silicon-based thin film layer, but less than the sum of the thicknesses of the third intrinsic amorphous silicon thin film layer and the boron-doped silicon-based thin film layer;
[0061] Specifically, when a laser is used to groove the back of the silicon wafer, the groove depth needs to be controlled so that the local boron-doped silicon-based thin film layer 7 is ablated but the surface of the silicon wafer cannot be damaged. That is, the groove depth is greater than the thickness of the boron-doped silicon-based thin film layer 7 but less than the sum of the thickness of the third intrinsic amorphous silicon thin film layer 6 and the boron-doped silicon-based thin film layer 7. Figure 4 As shown; therefore, the laser wavelength is between 200nm-500nm, the laser type is one of nanosecond laser, femtosecond laser or picosecond laser, the frequency is 10E12HZ-10E19HZ, the laser slot width is 10um-100um, and the interval between adjacent laser slots is 30-300um.
[0062] For this type of laser, since the boron element is doped in the boron-doped silicon-based thin film layer 7, the coefficient of the laser in the short-wave band will be larger than that of the intrinsic amorphous silicon. Therefore, most of the laser energy is absorbed by the boron-doped silicon-based thin film layer 7, causing the local boron-doped silicon-based thin film layer 7 to instantly vaporize and leak out the intrinsic amorphous silicon underneath; the fourth intrinsic amorphous silicon thin film layer 8 will not be damaged too much.
[0063] Step S5: Clean the surface of the silicon wafer to remove pollutants and oxides generated during the laser ablation process.
[0064] Since silicon oxide and some contaminants will be produced on the surface of the third intrinsic amorphous silicon thin film layer 6 underneath after local laser ablation, the silicon wafer needs to be transferred to a wet process equipment for cleaning after local laser ablation, and the surface of the silicon wafer is cleaned with a hydrofluoric acid aqueous solution to remove the contaminants and oxides on the surface of the third intrinsic amorphous silicon thin film layer 6; in addition, since the amorphous silicon on the front and back sides will not react with the hydrofluoric acid aqueous solution, the film will not be etched, and only the surface of the film will be cleaned.
[0065] Step S6, depositing a fourth intrinsic amorphous silicon thin film layer and a second phosphorus-doped silicon-based thin film layer on the back side of the silicon wafer;
[0066] A fourth intrinsic amorphous silicon thin film layer 8 and a second phosphorus-doped silicon-based thin film layer 9 are deposited on the back of the silicon wafer by chemical vapor deposition.
[0067] Since the laser will ablate the local third intrinsic amorphous silicon film layer 6, therefore, depositing the fourth intrinsic amorphous silicon film layer 8 can enhance the passivation effect of the third intrinsic amorphous silicon film layer at the laser grooved portion; the thickness of the fourth intrinsic amorphous silicon film layer 8 is 4n-10nm, and the refractive index is between 3.5-4.4.
[0068] It should be noted that the second phosphorus-doped silicon-based thin film layer 9 can be a phosphorus-doped amorphous silicon thin film or a phosphorus-doped microcrystalline silicon thin film or a phosphorus-doped microcrystalline silicon oxide thin film. This application does not make specific limitations and all are within the protection scope of this application. The purpose of the second phosphorus-doped silicon-based thin film layer 9 is to further provide a field passivation effect for the surface and improve the battery conversion efficiency; the thickness of this film layer is 4n-30nm, and the refractive index is between 2.2-4.5.
[0069] It should be further explained that, although the second phosphorus-doped silicon-based thin film layer 9 also has a passivation effect, the passivation principles of the second phosphorus-doped silicon-based thin film layer 9 and the intrinsic amorphous silicon thin film are different. The intrinsic amorphous silicon is interface passivation, while the phosphorus-doped silicon-based thin film is field passivation; therefore, the present application adopts chemical vapor deposition to deposit the fourth intrinsic amorphous silicon thin film layer 8 on the back of the silicon wafer, which plays a role in supplementing the thickness of the intrinsic amorphous silicon and enhancing the interface passivation effect.
[0070] Step S7, coating a layer of alkali corrosion resistant wet film material on the laser slotted area, wherein the width of the wet film material is 2um-20um greater than the laser slotted width;
[0071] A layer of alkali corrosion resistant wet film material 10 is coated on the laser slotted area by inkjet printing or screen printing. Figure 5 As shown, the material is resistant to etching by common alkaline solutions such as ammonia, potassium hydroxide, and sodium hydroxide, but is easily cleaned by common acids such as hydrochloric acid, phosphoric acid, and hydrofluoric acid. At the same time, the width of the wet film material 10 is 30-120um, which is 2um-20um wider than the laser groove width, so as to completely protect the second phosphorus-doped silicon-based thin film layer 9 corresponding to the laser groove area from being etched by subsequent alkaline solutions.
[0072] Among them, the main component of the wet film material 10 is a mixture of acrylic polyester and acrylic copolymer resin, and the mass ratio of acrylic polyester to acrylic copolymer resin can be arbitrarily adjusted, both between 10-90%; for example, when the mass ratio of acrylic polyester is 20%, the corresponding mass ratio of acrylic copolymer resin is 80%; when the mass ratio of acrylic polyester is 30%, the corresponding mass ratio of acrylic copolymer resin is 70%, and the sum of the mass ratios of the two is 100%.
[0073] Step S8, cleaning the silicon wafer with an alkaline solution to remove the second intrinsic amorphous silicon thin film layer on the front side of the silicon wafer and the second phosphorus-doped silicon-based thin film layer and the fourth intrinsic amorphous silicon thin film layer on the back side of the silicon wafer that are not protected by the wet film material; cleaning the silicon wafer with an acid solution to remove the silicon nitride thin film layer on the front side of the silicon wafer and the wet film material on the back side of the silicon wafer;
[0074] Specifically, the sample is placed in a common alkaline solution such as ammonia water, potassium hydroxide, and sodium hydroxide for cleaning. Since the second intrinsic amorphous silicon thin film layer 5 on the front side of the silicon wafer and the second phosphorus-doped silicon-based thin film layer 9 and the fourth intrinsic amorphous silicon thin film layer 8 on the back side that are not protected by the wet film material 10 are not resistant to alkali corrosion, they will be removed; while the boron-doped silicon-based thin film layer 7 is retained due to its excellent acid and alkali corrosion resistance. At this time, the silicon nitride thin film layer 4 is leaked on the front side, and the back side is the boron-doped silicon-based thin film layer 7 and the second phosphorus-doped silicon-based thin film layer 9 protected by the wet film and the unetched wet film.
[0075] The sample is then placed in a common acid such as hydrochloric acid, phosphoric acid, and hydrofluoric acid for cleaning. Since the wet film material 10 on the back is etched by the acid, the second phosphorus-doped silicon-based film layer 9 is exposed on the back, forming an interdigitated structure of boron-doped silicon-based films and phosphorus-doped silicon-based films. Finally, the sample is cleaned with a hydrofluoric acid aqueous solution. Since the silicon films are resistant to hydrofluoric acid etching and are retained, the front silicon nitride film layer 4 will be etched by hydrofluoric acid. After this step, a phosphorus-doped silicon-based film appears on the front, and an interdigitated structure of boron-doped silicon-based films and phosphorus-doped silicon-based films arranged at intervals is realized on the back, as shown in FIG. Figure 6shown.
[0076] It should be noted that the present application obtains a finger-like structure of spaced boron-doped silicon-based films and phosphorus-doped silicon-based films by coating a layer of alkali-corrosion-resistant wet film material 10 on the laser-grooved area, and then removing the second phosphorus-doped silicon-based film layer 9 and the fourth intrinsic amorphous silicon film layer 8 on the back side that are not protected by the wet film material 10 by an alkaline solution, and then removing the wet film material 10 by an acid solution. Compared with laser ablation of the second phosphorus-doped silicon-based film layer 9 and the fourth intrinsic amorphous silicon film layer 8 that are not protected by the wet film material 10, the present application reduces damage to the boron-doped silicon-based film layer 7, thereby reducing damage to the silicon wafer and improving the conversion efficiency of the battery.
[0077] Step S9, depositing a thin film interference layer on the front side of the silicon wafer;
[0078] The thin film interference layer 11 includes but is not limited to one or more laminated thin films selected from the group consisting of a silicon nitride thin film layer, a silicon oxynitride thin film layer and a silicon oxide thin film layer. The thickness of the thin film interference layer 11 is between 60nm and 200nm, the refractive index of the thin film is between 1.4 and 3.0, and the refractive index of the thin film interference layer 11 increases from top to bottom.
[0079] Specifically, a thin film interference layer 11 is deposited on the front side of the silicon wafer by chemical vapor deposition, wherein the thin film interference layer 11 includes but is not limited to one or more laminated thin films selected from the group consisting of a silicon nitride thin film layer, a silicon oxynitride thin film layer, and a silicon oxide thin film layer, such as Figure 7 As shown; its purpose is to further reduce the reflectivity of the silicon wafer surface by using the thin film interference principle.
[0080] Step S10, depositing a transparent conductive film layer on the back side of the silicon wafer;
[0081] A transparent conductive film layer 12 is deposited on the back of the silicon wafer by magnetron sputtering or reactive plasma deposition. The obtained silicon wafer structure is as follows: Figure 8 As shown, the film can be a conductive oxide containing indium or a conductive oxide not containing indium, the film thickness is 30nm-300nm, and the film refractive index is between 1.7-3.0.
[0082] The main function of this film is to increase the surface conductivity of the silicon film, increase the back reflection of long-wave incident light, and reduce the contact resistance of the metal interface.
[0083] Step S11, using laser to isolate and scribe the transparent conductive film layer to block lateral conduction between the second phosphorus-doped silicon-based film layer and the boron-doped silicon-based film layer;
[0084] Specifically, laser is used to isolate and scribe the transparent conductive film layer 12. The scribe line is located between the phosphorus-doped silicon film and the boron-doped silicon film prepared previously. The purpose is to cut off the lateral conduction between the two films to avoid leakage and reduce the conversion efficiency of the solar cell.
[0085] The width of the laser scribing in this step is 1um-50um. Since the lateral conductivity between the two thin films needs to be cut off, the depth of the laser scribing should be greater than the thickness of the transparent conductive film layer 12, and the laser scribing should not damage the third intrinsic amorphous silicon film layer 6. Fig. 9 As shown, the laser wavelength is between 200nm-500nm, the laser type is one of nanosecond laser, femtosecond laser or picosecond laser, and the frequency is 10E12HZ-10E19HZ.
[0086] Step S12, preparing a metal electrode on the back of the silicon wafer, the metal electrode corresponding to the second phosphorus-doped silicon-based thin film layer is the negative electrode of the solar cell, and the metal electrode corresponding to the boron-doped silicon-based thin film layer is the positive electrode of the solar cell.
[0087] Conductive paste is printed on the back of the silicon wafer using screen printing technology to form a metal electrode 1. The conductive paste can be silver paste, copper paste, silver-coated copper paste, carbon paste, etc. The metal electrode 1 includes a main gate and a secondary gate. The gate line width of each metal electrode 1 cannot be greater than the width of the phosphorus-doped silicon film or the boron-doped silicon film under the gate line to avoid leakage, and the metal electrode 1 above the phosphorus-doped silicon film cannot be connected to the gate line electrode above the boron-doped silicon film, that is, the gate line of the metal electrode 1 cannot cross the laser scribing line to avoid short circuits and reduce the conversion efficiency of the solar cell. Fig.10 As shown, the width of the gate line electrode on the phosphorus-doped silicon-based film is 5um-95um, the width of the electrode above the boron-doped silicon-based film is 10um-290um, and the height of the gate line electrode is 1um-30um; the method for preparing the gate line electrode can be screen printing or inkjet printing conductive paste technology.
[0088] It should be noted that the metal electrode 1 corresponding to the phosphorus-doped silicon-based thin film region is the negative electrode of the solar cell, and the boron-doped silicon-based thin film region is the positive electrode of the battery. The positive and negative electrodes are strictly prohibited from being connected to each other.
[0089] In summary, the present invention proposes a relatively low-cost and simple process technology route. First, it utilizes the convenience of laser ablation to prepare graphics, and also adopts the inkjet mask method to replace the one-step laser ablation method to avoid the disadvantage of multiple laser etching that damages the intrinsic amorphous silicon layer to reduce the passivation effect. Finally, it introduces an efficient and simple process technology route, which is expected to promote the large-scale mass production of high-efficiency back-junction back-contact heterojunction solar cells. Specifically, the present invention coats a layer of alkali corrosion-resistant wet film material 10 on the laser grooved area by an inkjet mask method, and then removes the second phosphorus-doped silicon-based thin film layer 9 and the fourth intrinsic amorphous silicon thin film layer 8 on the back side that are not protected by the wet film material 10 by an alkaline solution, and then removes the wet film material 10 by an acid solution to obtain an interdigitated structure of boron-doped silicon-based thin films and phosphorus-doped silicon-based thin films. The present invention adopts alkali-resistant wet film protection combined with a wet etching process, which reduces the damage to the boron-doped silicon-based thin film layer 7 compared to directly laser ablating the second phosphorus-doped silicon-based thin film layer 9 and the fourth intrinsic amorphous silicon thin film layer 8, avoids the risk of intrinsic amorphous silicon passivation failure caused by laser ablation, and thus reduces the damage to the silicon wafer. damage, thereby improving the conversion efficiency of the battery. Compared with the three-step laser ablation method, one laser process is also reduced. The application of the technology of the present invention can more efficiently mass-produce back-junction and back-contact heterojunction solar cells; in addition, the present application improves the interface passivation effect and field passivation effect of the laser grooved area by depositing a fourth intrinsic amorphous silicon thin film layer 8 and a second phosphorus-doped silicon-based thin film layer 9, respectively, thereby improving the conversion efficiency of the battery. Moreover, the present application adopts an inkjet mask method to coat a layer of alkali corrosion-resistant wet film material 10 in the laser grooved area to obtain a forked finger structure of spaced boron-doped silicon-based thin films and phosphorus-doped silicon-based thin films, which does not damage the passivation effect of the intrinsic amorphous silicon thin film layer in the laser grooved area. More importantly, the present application deposits a first intrinsic amorphous silicon thin film layer 2, a first phosphorus-doped silicon-based thin film layer 3, a silicon nitride thin film layer 4 and a second intrinsic amorphous silicon thin film layer 5 in sequence on the front side of the silicon wafer; the second intrinsic amorphous silicon thin film layer 5 is used to prevent the front side of the silicon wafer from being corroded by an acid solution, so that a hydrofluoric acid aqueous solution can be used to clean the pollutants and oxides in the laser grooved area, and the silicon nitride thin film layer 4 on the front side of the silicon wafer prevents the front side of the silicon wafer from being corroded by an alkaline solution, so that a layer of alkali-corrosion-resistant wet film material can be coated on the laser grooved area accordingly, thereby avoiding the disadvantage of multiple laser etching causing damage to the intrinsic amorphous silicon layer to reduce the passivation effect.
[0090] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation to the invention.
[0091] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials, or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.
[0092] Obviously, the described embodiments are only a part of the embodiments of the present application, rather than all the embodiments. Mentioning "embodiment" in this article means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present embodiment application. The appearance of this phrase in various positions in the specification is not necessarily the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It can be explicitly and implicitly understood by those skilled in the art that the embodiments described herein can be combined with other embodiments. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0093] Although the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the claims and their equivalents.
Claims
1. A method for preparing a back-contact heterojunction solar cell, characterized in that: The specific steps include: Pre-treating the surface of the silicon wafer; Depositing a first intrinsic amorphous silicon thin film layer, a first phosphorus-doped silicon-based thin film layer, a silicon nitride thin film layer, and a second intrinsic amorphous silicon thin film layer in sequence on the front side of the silicon wafer; Depositing a third intrinsic amorphous silicon thin film layer and a boron-doped silicon-based thin film layer in sequence on the back side of the silicon wafer; The back side of the silicon wafer is grooved by laser, wherein the groove depth is greater than the thickness of the boron-doped silicon-based thin film layer, but less than the sum of the thickness of the third intrinsic amorphous silicon thin film layer and the boron-doped silicon-based thin film layer; Depositing a fourth intrinsic amorphous silicon thin film layer and a second phosphorus-doped silicon-based thin film layer on the back side of the silicon wafer; A layer of alkali corrosion-resistant wet film material is coated on the laser slotted area, and the width of the wet film material is 2um to 20um greater than the laser slotted width; The silicon wafer is cleaned with an alkaline solution to remove the second intrinsic amorphous silicon thin film layer on the front side of the silicon wafer and the second phosphorus-doped silicon-based thin film layer and the fourth intrinsic amorphous silicon thin film layer on the back side of the silicon wafer that are not protected by the wet film material; the silicon wafer is cleaned with an acid solution to remove the silicon nitride thin film layer on the front side of the silicon wafer and the wet film material on the back side of the silicon wafer; Depositing a thin film interference layer on the front side of the silicon wafer, wherein the thin film interference layer comprises one or more laminated thin films of a silicon nitride thin film layer, a silicon oxynitride thin film layer and a silicon oxide thin film layer, the thickness of the thin film interference layer is 60nm to 200nm, the refractive index of the thin film is between 1.4 and 3.0, and the refractive index of the thin film interference layer increases from top to bottom; Depositing a transparent conductive film layer on the back of the silicon wafer; Using laser to isolate and scribe the transparent conductive film layer to block the lateral conduction between the second phosphorus-doped silicon-based film layer and the boron-doped silicon-based film layer; A metal electrode is prepared on the back of the silicon wafer. The metal electrode corresponding to the second phosphorus-doped silicon-based thin film layer is the negative electrode of the solar cell, and the metal electrode corresponding to the boron-doped silicon-based thin film layer is the positive electrode of the solar cell.
2. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: The step of using laser to groove the back of the silicon wafer, wherein the groove depth is greater than the thickness of the boron-doped silicon-based thin film layer and less than the sum of the thickness of the third intrinsic amorphous silicon thin film layer and the boron-doped silicon-based thin film layer, comprises: The silicon wafer surface is cleaned to remove contaminants and oxides generated during the laser ablation process.
3. The method for preparing a back-contact heterojunction solar cell according to claim 2, characterized in that: The step of cleaning the surface of the silicon wafer to remove pollutants and oxides generated during the laser ablation process specifically includes: The silicon wafer is transferred to a wet process device for cleaning, and the surface of the silicon wafer is cleaned with a hydrofluoric acid aqueous solution to remove pollutants and oxides on the surface of the silicon wafer.
4. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: The phosphorus-doped silicon-based film layer is a phosphorus-doped amorphous silicon film layer, a phosphorus-doped microcrystalline silicon film layer, or a phosphorus-doped microcrystalline silicon oxide film; the boron-doped silicon-based film layer is a boron-doped amorphous silicon film layer, a boron-doped microcrystalline silicon film layer, or a boron-doped microcrystalline silicon oxide film.
5. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: The step of pre-treating the surface of the silicon wafer comprises: First, the double-sided silicon wafer is textured, and then the organic pollutants and metal ion pollutants on the surface of the silicon wafer are removed using acidic and alkaline solutions. Finally, the silicon wafer is immersed in a hydrofluoric acid aqueous solution to remove the oxide layer on the surface of the silicon wafer and is dried.
6. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: The wavelength of the laser used to groove the back of the silicon wafer is between 200nm and 500nm. The laser is a nanosecond laser, a femtosecond laser or a picosecond laser. The frequency is 10E12HZ to 10E19HZ. The width of the laser groove is 10um to 100um, and the interval between adjacent laser grooves is 30 to 300um.
7. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: The step of coating a layer of alkali corrosion resistant wet film material on the laser slotted area, wherein the width of the wet film material is 2 um to 20 um greater than the laser slotted width, specifically comprises: A layer of alkali corrosion-resistant wet film material is coated on the laser slotted area by inkjet printing or screen printing, and the width of the wet film material is 30 to 120 um.
8. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: The step of depositing a transparent conductive film layer on the back side of the silicon wafer specifically comprises: A transparent conductive film layer is deposited on the back of a silicon wafer by magnetron sputtering or reactive plasma deposition. The transparent conductive film layer is an indium-containing conductive oxide or an indium-free conductive oxide. The thickness of the transparent conductive film layer is 30nm to 300nm, and the refractive index of the film is between 1.7 and 3.
0.
9. The method for preparing a back-contact heterojunction solar cell according to claim 1, characterized in that: The wavelength of the laser used to isolate and scribe the transparent conductive film layer is between 200nm and 500nm, the laser type is one of nanosecond laser, femtosecond laser or picosecond laser, the frequency is 10E12HZ to 10E19HZ, and the width of the laser scribe is 1um to 50um.