A coaxial fiber heterojunction for realizing visible light catalysis and a preparation method thereof

Coaxial ZnO@CuO nanofiber structure was prepared through electrospinning technology, which solved the problems of uncontrollable microstructure of CuO/ZnO p-n heterojunction and low electron-hole separation efficiency, achieving more efficient photocatalytic performance and antibacterial effect .

CN118179516BActive Publication Date: 2024-11-12PEKING UNIV SCHOOL OF STOMATOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410351684.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-26
Publication Date
2024-11-12
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

The microstructure of the existing CuO/ZnO p-n heterojunction is uncontrollable and the electron-hole separation efficiency is low, which limits its application and photocatalytic properties in biomedicine.

Method used

Coaxial ZnO@CuO nanofibers were prepared by electrospinning technology to construct a controllable and stable coaxial structure p-n heterojunction, enlarging the contact interface and generating an internal electric field, and improving the dynamics of photogenerated charge carriers.

Benefits of technology

More efficient electron-hole separation is achieved, photocatalytic performance is improved, reactive oxygen species is generated for antibacterial purposes, and is suitable for complex immune microenvironment, such as infectious wound healing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118179516B_ABST
    Figure CN118179516B_ABST
Patent Text Reader

Abstract

The present invention uses electrostatic spinning and specific process parameters to prepare coaxial ZnO@CuO nanofibers to construct a controllable and stable coaxial structure p-n heterojunction. Therefore, based on this stable microstructure and favorable electronic structure, the ZnO@CuO heterojunction exhibits better photocatalytic performance than the original component. During the photocatalytic reaction, the active oxygen components that can be generated for antibacterial purposes include hydroxyl radicals and superoxide radicals, and the antibacterial effect of zinc oxide itself and the angiogenic effect of copper oxide are combined, so as to better cope with the complex immune microenvironment and promote the healing of infectious wounds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of photocatalysis, and in particular relates to a coaxial fiber heterojunction for realizing visible light catalysis and a preparation method thereof. Background Art

[0002] Energy shortage and environmental pollution have made people urgently develop environmentally friendly and renewable technologies for green energy production and environmental problem remediation. Semiconductor-based photocatalytic technology can directly use solar energy to produce valuable chemical fuels and degrade harmful pollutants, highlighting its advantages among the various technologies proposed. At the same time, active oxygen can be produced in the photocatalytic reaction, so it also has great potential in antibacterial aspects. Various strategies have been proposed to effectively separate photogenerated electron-hole pairs in semiconductor photocatalysts, such as through doping, metal loading, and introduction of heterojunctions. Among the proposed strategies, heterojunctions have been proven to be one of the most promising methods for preparing advanced photocatalysts because it is effective for the spatial separation of electron-hole pairs.

[0003] At present, the heterojunction with better separation of photogenerated electrons and holes in ordinary heterojunctions is the staggered gap heterojunction, in which the conduction band and valence band energy levels of semiconductor A are higher than the corresponding energy levels of semiconductor B. Therefore, under light irradiation, the photogenerated electrons will transfer to semiconductor B, while the photogenerated holes will migrate to semiconductor A, resulting in the spatial separation of electron-hole pairs. At the same time, the coaxial structure has a larger contact interface, which can further improve the separation efficiency of electron-hole pairs. For example, studies have shown that the photocatalytic hydrogen production efficiency of zinc oxide / cadmium sulfide is higher than that of single zinc oxide and cadmium sulfide.

[0004] However, the enhancement of electron-hole separation in staggered gap heterojunctions is not sufficient to overcome the ultrafast electron-hole recombination on semiconductors. Therefore, the concept of pn heterojunction photocatalysts has been proposed, which can accelerate the migration of electrons and holes on the heterojunction by providing an additional electric field, thereby improving the photocatalytic performance. The currently developed pn heterojunctions such as NiS / CdS, MoS2 / CdS, and NiO / TiO2 have limited their application in biomedicine due to the addition of metal elements such as nickel and cadmium. Therefore, the use of semiconductor materials with good biocompatibility and strong antibacterial properties to construct pn heterojunctions will have great potential in clinical transformation. ZnO is generally considered to be a typical n-type semiconductor with a wide bandgap (Eg = 3.37 eV), which makes it photocatalytically active in the ultraviolet (UV) region. In other words, most of the sunlight cannot be used, which seriously restricts the efficiency of ZnO photocatalysts. Copper oxide materials have the advantages of narrow bandgap, visible light response, non-toxicity, and stable performance, and are one of the promising candidate materials for the preparation of ZnO pn heterojunctions. Several studies have been reported on the preparation of CuO / ZnO pn heterojunctions to study gas sensors or photocatalytic activity. However, the complex synthesis strategies used in these studies will lead to uncontrollable microstructures of CuO / ZnO pn heterojunctions. In addition, for the CuO / ZnO pn heterojunction photocatalytic system, revealing the photocatalytic mechanism based on detailed experiments is still lacking and challenging.

[0005] The currently developed NiS / CdS, MoS2 / CdS, NiO / TiO2 and other pn heterojunctions have limited their application in biomedicine due to the addition of metal elements such as nickel and cadmium. The currently synthesized CuO / ZnO pn heterojunction is a simple doping, has no specific structure, uncontrollable microstructure, and low electron-hole separation efficiency. Summary of the invention

[0006] In view of the shortcomings of the above-mentioned prior art, a method for preparing a coaxial fiber heterojunction for realizing visible light catalysis is provided, in which coaxial ZnO@CuO nanofibers are prepared by electrospinning to construct a controllable and stable coaxial structure pn heterojunction, thereby increasing the contact interface of the pn heterojunction and further improving the electron-hole separation efficiency.

[0007] The present invention provides a method for preparing a coaxial fiber heterojunction for realizing visible light catalysis, comprising the following steps:

[0008] (1) Preparing a spinning precursor solution: dissolving zinc salt and copper salt in an organic solvent respectively, adding polyvinyl pyrrolidone, and stirring to obtain precursor solutions 1 and 2;

[0009] (2) Preparation of coaxial ZnO@CuO precursor fibers by electrospinning: Precursor solutions 1 and 2 were placed in syringe pumps respectively and prepared using a coaxial electrospinning process, wherein precursor 1 was the outer layer and precursor solution 2 was the inner layer; the ratio of the outer layer flow rate to the inner layer flow rate was 5:1;

[0010] (3) Preparation of ZnO@CuO coaxial fiber heterojunction by high-temperature calcination: After 8 h of electrospinning, the fiber was transferred to a muffle furnace and heated to 400-600 °C. After keeping the temperature for 3-6 h, the fiber was cooled naturally to obtain a ZnO@CuO coaxial fiber heterojunction.

[0011] In step (1), the zinc salt is zinc acetate, the copper salt is copper nitrate, the organic solvent is N,N-dimethylformamide, the ratio of zinc salt, copper salt and organic solvent is 1g: (8-30)mL; the molar ratio of zinc salt to copper salt is: (1-3): 1; the mass ratio of zinc salt, copper salt and polyvinyl pyrrolidone is 1: 1-2;

[0012] The electrospinning conditions in step (2) were as follows: voltage 13 kV, outer layer flow rate 0.1 ml / min, inner layer flow rate 0.02 ml / min, shaft speed 600 rpm, and electrospinning distance 15 cm.

[0013] In step (3), the heating rate is 5°C / min, the calcination temperature is 500°C, and the holding time is 4h.

[0014] The ZnO@CuO coaxial fiber heterojunction prepared by the above preparation method can be used as a photocatalyst.

[0015] In the present invention, coaxial ZnO@CuO nanofibers are prepared by electrospinning and specific process parameters to construct a controllable and stable coaxial structure pn heterojunction. The pn heterojunction contact interface is enlarged to further improve the electron-hole separation efficiency. And at the interface of the ZnO@CuO pn heterojunction, due to the difference in Fermi level, an internal electric field is generated. Therefore, the reverse transfer of electrons and holes at the pn heterojunction interface can be easily achieved, thereby improving the dynamics of photogenerated charge carriers. Therefore, on the basis of this stable microstructure and favorable electronic structure, the ZnO@CuO heterojunction exhibits better photocatalytic performance than the original component. In the process of photocatalytic reaction, the active oxygen components that can be generated for antibacterial are hydroxyl radicals and superoxide radicals, and the antibacterial effect of zinc oxide itself and the angiogenic effect of copper oxide are combined, so as to better cope with the complex immune microenvironment and promote the healing of infectious wounds. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0017] Figure 1 It is the SEM picture of the product of comparative example 1-3 and embodiment 1;

[0018] Figure 2 TEM image and XRD image of the product of Example 1;

[0019] Figure 3 The EPR test results of Example 1 and Comparative Example 4 are shown in FIG. DETAILED DESCRIPTION

[0020] The invention is further described below in conjunction with specific examples. It should be noted that the following examples are only used to illustrate the present invention and are not intended to limit the technical solutions described in the present invention. All technical solutions and improvements that do not depart from the spirit and scope of the present invention should be included in the scope of the claims of the present invention.

[0021] Example 1

[0022] (1) Preparation of spinning precursor solution: Weigh 1 g zinc acetate dihydrate and dissolve it in 10 ml N, N-dimethylformamide, then weigh 1.6 g polyvinyl pyrrolidone and add it to the solution, and stir it magnetically at room temperature for 6 h to obtain precursor solution 1. Weigh 0.4 g copper nitrate trihydrate and dissolve it in 10 ml N, N-dimethylformamide, then weigh 0.55 g polyvinyl pyrrolidone and add it to the solution, and stir it magnetically at room temperature for 6 h to obtain precursor solution 2.

[0023] (2) Preparation of coaxial ZnO@CuO precursor fibers by electrospinning: Precursor solutions 1 and 2 were placed in 20 ml syringe pumps respectively and prepared using a coaxial electrospinning process, where precursor 1 was the outer layer and precursor solution 2 was the inner layer. The electrospinning conditions were voltage 13 kV, outer layer flow rate 0.1 ml / min, inner layer flow rate 0.02 ml / min, shaft speed 600 rpm, and electrospinning distance 15 cm.

[0024] (3) Preparation of ZnO@CuO coaxial fiber heterojunction by high temperature calcination: After electrospinning for 8 h in step 2, the electrospun membrane on the aluminum foil was collected and transferred to a crucible and muffle furnace. The temperature was raised to 500 °C at a rate of 5 °C / min, kept at this temperature for 4 h, and then cooled naturally. The ZnO@CuO coaxial fiber heterojunction was obtained.

[0025] Comparative Example 1

[0026] The outer layer flow rate in step (2) of Example 1 was set to 0.04 ml / min, and the rest was the same as Example 1.

[0027] Comparative Example 2

[0028] The outer layer flow rate in step (2) of Example 1 was set to 0.06 ml / min, and the rest was the same as Example 1.

[0029] Comparative Example 3

[0030] The outer layer flow rate in step (2) of Example 1 was set to 0.08 ml / min, and the rest was the same as Example 1.

[0031] Comparative Example 4

[0032] Precursor solutions 1 and 2 were mixed for electrospinning, and the rest was the same as in Example 1.

[0033] The products of Example 1 and Comparative Examples 1-3 were observed using SEM.

[0034] Instructions attached Figure 1 The product morphology of Example 1 and Comparative Examples 1-3 is shown in the figure. After exploring the electrospinning parameters, it was found that the spinning flow rate ratio of the inner and outer layers would affect the nano-morphology. Combined with SEM observation, (a)-(d) are the product images of Comparative Examples 1-3 and Example 1, that is, the spinning flow rate ratio of the inner and outer layers is 1:2, 1:3, 1:4, and 1:5, respectively. It was found that when the flow rate ratio of the inner and outer layers is 1:5 (Example 1), a fiber morphology appears, while no coaxial fiber structure is obtained in Comparative Examples 1-3.

[0035] The morphology of the ZnO@CuO coaxial fiber of Example 1 was observed by TEM, and its crystal structure was tested by XRD. Figure 2 As shown in A, the inner and outer layer structures of the TEM image are clearly visible. Figure 2 B), CuO characteristic peaks were observed at 2θ of 35.54°, 38.70°, etc., and ZnO characteristic peaks were observed at 31.7°, 34.4°, 36.2°, 47.5°, 56.6°, 62.9°, etc.

[0036] The EPR spin trapping experiment was conducted on the ZnO@CuO coaxial fiber photocatalytic system in Example 1, and the ZnO / CuO nanofiber without coaxial structure produced by uniaxial spinning of ZnO and CuO simply mixed under the same conditions in Comparative Example 4 was tested to detect the signal strength of hydroxyl radicals generated under visible light response. EPR experimental results ( Figure 3 ) It can be seen that the hydroxyl radical signal captured by the scavenger in the ZnO@CuO coaxial fiber is stronger under visible light irradiation, and the coaxial structure of the ZnO@CuO heterojunction of the present invention has better visible light photocatalytic performance than the unstructured ZnO / CuO.

[0037] The principles, steps, etc. not explicitly described in the present invention are all obtainable by those skilled in the art through conventional technical means, and therefore will not be described in detail. Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a coaxial fiber heterojunction for realizing visible light catalysis, characterized in that: The following steps are involved: (1) preparing a spinning precursor solution: dissolving a zinc salt and a copper salt in an organic solvent respectively, adding polyvinyl pyrrolidone, and stirring to obtain precursor solutions 1 and 2; (2) Preparation of coaxial ZnO@CuO precursor fibers by electrospinning: Precursor solutions 1 and 2 were placed in syringe pumps respectively and prepared by coaxial electrospinning process, wherein precursor 1 was the outer layer and precursor solution 2 was the inner layer; the ratio of the outer layer flow rate to the inner layer flow rate was 5:1; (3) Preparation of ZnO@CuO coaxial fiber heterojunction by high temperature calcination: After 8 hours of electrospinning, the fiber was transferred to a muffle furnace, heated to 400-600°C, kept at this temperature for 3-6 hours, and then cooled naturally to obtain a ZnO@CuO coaxial fiber heterojunction; The electrospinning conditions in step (2) are as follows: voltage 13 kV, outer layer flow rate 0.1 mL / min, inner layer flow rate 0.02 mL / min, shaft speed 600 rpm, and electrospinning distance 15 cm.

2. The method for preparing a coaxial fiber heterojunction for realizing visible light catalysis according to claim 1, characterized in that: In step (1), the zinc salt is zinc acetate, the copper salt is copper nitrate, and the organic solvent is N,N-dimethylformamide.

3. The method for preparing a coaxial fiber heterojunction for realizing visible light catalysis according to claim 1 or 2, characterized in that: The ratio of zinc salt, copper salt and organic solvent is 1g:(8-30)mL; the molar ratio of zinc salt and copper salt is (1-3):1; the mass ratio of zinc salt, copper salt and polyvinyl pyrrolidone is 1:1-2.

4. The method for preparing a coaxial fiber heterojunction for realizing visible light catalysis according to claim 1, characterized in that: In step (3), the heating rate is 5°C / min, the calcination temperature is 500°C, and the holding time is 4h.

5. A coaxial fiber heterojunction for achieving visible light photocatalysis prepared by the preparation method according to any one of claims 1 to 4.

6. Use of the coaxial fiber heterojunction for realizing visible light catalysis as claimed in claim 5 as a photocatalyst.