A preparation method and application of modified ultrafine titanium dioxide
By using organic templates to prepare rutile nano-titanium dioxide in ceramic glazes and adding silane coupling agents to generate silver-loaded nanoparticles, the problems of low antibacterial efficiency and poor dispersion of nano-titanium dioxide under high temperature conditions are solved, and efficient Antibacterial and mechanical strength improvement.
Patent Information
- Application Number
- CN202410369001.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-03-28
AI Technical Summary
The crystal form of commercially available nano-titanium dioxide changes under high temperature conditions, resulting in unsatisfactory antibacterial efficiency under ultraviolet and visible light conditions, and its dispersion and mechanical strength in ceramic glazes are insufficient, making it difficult to be widely used.
A specific organic template is used to prepare rutile titanium dioxide nanoparticles, and silver-loaded nanoparticles are generated through the complex reduction method, which is combined with modification by a silane coupling agent to improve the antibacterial properties and mechanical strength of the glaze.
Under ultraviolet and visible light conditions, the antibacterial rate of the glaze was increased to 99.9%, the mechanical strength and dispersion of ceramic materials were improved, and the overall performance of the glaze was improved.
Smart Images

Figure BDA0004764976480000101 
Figure BDA0004764976480000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramics, and in particular relates to a preparation method and application of modified ultrafine titanium dioxide. Background Art
[0002] Daily necessities made of ceramic materials have also developed rapidly. In order to improve the surface performance of ceramic products, a layer of glaze needs to be applied on their surface. Glaze is a kind of silicate. The glaze applied on ceramics is generally made of quartz, feldspar, and clay. After grinding and adding water, it is applied to the surface of the body and melted by roasting at a certain temperature. When the temperature drops, a thin glass layer is formed on the surface of the ceramic. With the development of society and scientific progress, people have higher and higher requirements for the quality of ceramic products. For ceramic products, the quality of the glaze is one of the key factors affecting its quality. In addition to being related to the characteristics of the glaze slurry and the glazing process, the quality of the glaze of ceramic products is also related to the type of additives used.
[0003] Nano-titanium dioxide has the advantages of good stability, high photocatalytic activity, low price and non-toxicity. It has begun to be used in the production of self-cleaning ceramics, which is environmentally friendly and safe, and improves the quality of life. However, ceramics on the market that add nano-titanium dioxide often use high-quality glazed tiles as the base. They are high-end products with high prices and are difficult to popularize. The market is small. Most of the daily-use ceramic products on the market are ordinary quality, and the quality of the ceramic body is not high. This requires a layer of high-quality glaze on the surface of the daily-use ceramic body, which has certain self-cleaning properties, to ensure low costs and facilitate market promotion and use. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation method and application of modified ultrafine titanium dioxide. The modified ultrafine titanium dioxide can be used as a glaze additive to improve the quality of ordinary quality ceramic bodies and improve the antibacterial and mechanical strength properties of the glaze.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing modified ultrafine titanium dioxide, the preparation method comprising the following steps:
[0007] (1) mixing 7.5-8.2 parts by volume of ethanol and 10 parts by volume of tetraethyl titanate, adjusting the pH to 4-5, to obtain a first mixed solution; mixing the template with 7.5-8.2 parts by volume of ethanol, 2.1-2.4 parts by volume of water, 2.8-3.2 parts by volume of glacial acetic acid and 0.2-0.5 parts by volume of a silane coupling agent to obtain a second mixed solution; slowly dropping the second mixed solution into the first mixed solution to form a gel, and aging for 8-10 hours to obtain a nano titanium dioxide gel;
[0008] The preparation method of the template agent is as follows: cetyl trimethyl ammonium chloride, PEG-300 and octyl trimethyl ammonium bromide in a molar ratio of 1.2-1.5:3-3.5:0.6-0.9 are mixed, the temperature is raised to 63-65° C., and the reaction is stirred for 3-5 hours;
[0009] (2) After the nano-titanium dioxide gel is dried, it is placed in a tube furnace at 900-950° C. and calcined for 1-2 hours to obtain rutile nano-titanium dioxide;
[0010] (3) dispersing 100 parts by mass of rutile nano-titanium dioxide and 2-5 parts by mass of silver nitrate in 500 parts by mass of water, mixing them evenly to obtain a third mixed solution, mixing 1 part by volume of the third mixed solution with 12-14 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a first microemulsion; mixing 1 part by volume of an ascorbic acid aqueous solution with 12-14 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a second microemulsion; dropping the second microemulsion into the first microemulsion, stirring for 1-2 hours after the dropping is complete, to obtain a mixture;
[0011] (4) Washing the mixture, centrifuging and vacuum drying to obtain modified ultrafine titanium dioxide.
[0012] Furthermore, the concentration of the ascorbic acid aqueous solution is 10-15 mg / L.
[0013] Furthermore, the preparation method of the sodium dioctyl sulfonate dibutyrate solution is: dissolving sodium dioctyl sulfonate dibutyrate in isooctane to obtain a 0.12-0.14 mol / L sodium dioctyl sulfonate dibutyrate solution.
[0014] Furthermore, the molar ratio of the template to tetrabutyl titanate is 0.3-0.5:1.
[0015] Furthermore, the silane coupling agent is selected from one or more of silane coupling agent KH560, silane coupling agent KH550 and silane coupling agent KH570.
[0016] In order to improve the transparency of the glaze, further, the silane coupling agent is KH560.
[0017] Furthermore, in step (2), the drying temperature is 50-60° C. and the drying time is 2-3 hours.
[0018] Furthermore, in step (4), the mixture is washed 3-5 times with ethanol.
[0019] The invention also provides application of the modified ultrafine titanium dioxide prepared by the preparation method.
[0020] Furthermore, the modified ultrafine titanium dioxide is used in the preparation of ceramics.
[0021] Nano titanium dioxide is a photo-semiconductor material with photocatalytic function - photocatalyst. When it is applied to ceramic products, ceramic products need to be fired at high temperatures, and commercially available nano titanium dioxide is prone to crystal transformation at high temperatures, making its antibacterial effect under ultraviolet and visible light conditions unsatisfactory. The present invention prepares rutile nano titanium dioxide by using a specific organic template, and simultaneously prepares silver-loaded nano titanium dioxide, thereby improving the antibacterial rate of the glaze under ultraviolet and visible light conditions, up to 99.9%. It is speculated that the template prepared by the present invention has amphiphilicity, so that titanium dioxide has a good pore structure and a more uniform pore size, which is beneficial to improving the degradation efficiency of organic pollutants. At the same time, the structure of titanium dioxide is highly crystallized, which improves the thermal stability of the titanium dioxide structure. At the same time, silver-loaded nano titanium dioxide is prepared to synergistically exert antibacterial effects.
[0022] However, due to the small particle size of the ultrafine titanium dioxide prepared by using a template, the large number of atoms on the particle surface and the unsaturated atomic coordination, there are a large number of dangling bonds and unsaturated bonds, and water molecules are adsorbed on the particle surface, forming chemical bonds between particles and other factors, particle agglomeration is very likely to occur, which will reduce the antibacterial properties of antibacterial products and affect the compatibility with other components in the glaze. The present invention adds a silane coupling agent when preparing rutile nano titanium dioxide, which improves the dispersion of modified ultrafine titanium dioxide in the glaze, does not affect the antibacterial properties, and improves the mechanical strength of the ceramic material.
[0023] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0024] 1. The present invention adopts a sol-gel method or a hydrothermal method to prepare rutile nano-titanium dioxide, and modifies the surface of the nano-titanium dioxide, introduces an organic template, and then adopts a complex reduction method to generate silver nanoparticles. The modified ultrafine titanium dioxide of the present invention is applied to ceramic glazes to improve the antibacterial properties, mechanical strength and other properties of the glazes.
[0025] 2. The present invention prepares rutile nano-titanium dioxide by using a specific organic template and simultaneously prepares silver-loaded nano-titanium dioxide, thereby improving the antibacterial rate of the glaze under ultraviolet and visible light conditions to as high as 99.9%.
[0026] 3. The present invention adds a silane coupling agent when preparing rutile nano-titanium dioxide, thereby increasing the dispersion of the modified ultrafine titanium dioxide in the glaze and improving the mechanical strength of the ceramic material. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] This embodiment provides a method for preparing modified ultrafine titanium dioxide, the preparation method comprising the following steps:
[0030] (1) 7.9 parts by volume of ethanol and 10 parts by volume of tetraethyl titanate were mixed, and the pH was adjusted to 4.3 to obtain a first mixed solution; the template was mixed with 8.1 parts by volume of ethanol, 2.3 parts by volume of water, 3 parts by volume of glacial acetic acid and 0.4 parts by volume of a silane coupling agent to obtain a second mixed solution; the second mixed solution was slowly added dropwise to the first mixed solution to form a gel, and then aged for 9 hours to obtain a nano titanium dioxide gel;
[0031] The preparation method of the template agent is as follows: cetyl trimethyl ammonium chloride, PEG-300 and octyl trimethyl ammonium bromide in a molar ratio of 1.4:3.2:0.7 are mixed, the temperature is raised to 64°C, and the mixture is stirred for reaction for 4 hours;
[0032] (2) After the nano-titanium dioxide gel is dried, it is placed in a tube furnace at 930° C. and calcined for 1.5 h to obtain rutile nano-titanium dioxide;
[0033] (3) dispersing 100 parts by mass of rutile nano-titanium dioxide and 4 parts by mass of silver nitrate in 500 parts by mass of water, mixing them evenly to obtain a third mixed solution, mixing 1 part by volume of the third mixed solution with 13 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a first microemulsion; mixing 1 part by volume of an ascorbic acid aqueous solution with 13 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a second microemulsion; dropping the second microemulsion into the first microemulsion, stirring for 1.6 hours after the dropping is complete, to obtain a mixture;
[0034] (4) Washing the mixture, centrifuging and vacuum drying to obtain modified ultrafine titanium dioxide.
[0035] The concentration of the ascorbic acid aqueous solution is 12 mg / L.
[0036] The preparation method of the sodium dioctyl sulfonate dibutyrate solution is as follows: dissolving the sodium dioctyl sulfonate dibutyrate in isooctane to obtain a 0.13 mol / L sodium dioctyl sulfonate dibutyrate solution.
[0037] The molar ratio of the template to tetrabutyl titanate is 0.4:1.
[0038] The silane coupling agent is KH560.
[0039] The drying temperature in step (2) is 55° C. and the drying time is 2.6 h.
[0040] In the step (4), the mixture is washed 4 times with ethanol.
[0041] Example 2
[0042] This embodiment provides a method for preparing modified ultrafine titanium dioxide, the preparation method comprising the following steps:
[0043] (1) 7.5 parts by volume of ethanol and 10 parts by volume of tetraethyl titanate were mixed, and the pH was adjusted to 5 to obtain a first mixed solution; the template was mixed with 7.5 parts by volume of ethanol, 2.4 parts by volume of water, 2.8 parts by volume of glacial acetic acid and 0.5 parts by volume of a silane coupling agent to obtain a second mixed solution; the second mixed solution was slowly added dropwise to the first mixed solution to form a gel, and then aged for 8 hours to obtain a nano titanium dioxide gel;
[0044] The preparation method of the template agent is as follows: cetyl trimethyl ammonium chloride, PEG-300 and octyl trimethyl ammonium bromide in a molar ratio of 1.2:3.5:0.6 are mixed, the temperature is raised to 65° C., and the mixture is stirred for reaction for 3 hours;
[0045] (2) After the nano-titanium dioxide gel is dried, it is placed in a tube furnace and calcined for 2 hours at 950° C. to obtain rutile nano-titanium dioxide;
[0046] (3) dispersing 100 parts by mass of rutile nano-titanium dioxide and 2 parts by mass of silver nitrate in 500 parts by mass of water, mixing them evenly to obtain a third mixed solution, mixing 1 part by volume of the third mixed solution with 12 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a first microemulsion; mixing 1 part by volume of an ascorbic acid aqueous solution with 12 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a second microemulsion; dropping the second microemulsion into the first microemulsion, stirring for 2 hours after the dropping is complete, to obtain a mixture;
[0047] (4) Washing the mixture, centrifuging and vacuum drying to obtain modified ultrafine titanium dioxide.
[0048] The concentration of the ascorbic acid aqueous solution is 10 mg / L.
[0049] The preparation method of the sodium dioctyl sulfonate dibutyrate solution is as follows: dissolving the sodium dioctyl sulfonate dibutyrate in isooctane to obtain a 0.14 mol / L sodium dioctyl sulfonate dibutyrate solution.
[0050] The molar ratio of the template to tetrabutyl titanate is 0.5:1.
[0051] The silane coupling agent is KH550.
[0052] The drying temperature in step (2) is 60° C. and the drying time is 2 h.
[0053] In the step (4), the mixture is washed 5 times with ethanol.
[0054] Comparative Example 1
[0055] The difference between this comparative example and Example 1 is that no silver loading treatment is performed.
[0056] A method for preparing modified ultrafine titanium dioxide, the preparation method comprising the following steps:
[0057] (1) 7.9 parts by volume of ethanol and 10 parts by volume of tetraethyl titanate were mixed, and the pH was adjusted to 4.3 to obtain a first mixed solution; the template was mixed with 8.1 parts by volume of ethanol, 2.3 parts by volume of water, 3 parts by volume of glacial acetic acid and 0.4 parts by volume of a silane coupling agent to obtain a second mixed solution; the second mixed solution was slowly added dropwise to the first mixed solution to form a gel, and then aged for 9 hours to obtain a nano titanium dioxide gel;
[0058] The preparation method of the template agent is as follows: cetyl trimethyl ammonium chloride, PEG-300 and octyl trimethyl ammonium bromide in a molar ratio of 1.4:3.2:0.7 are mixed, the temperature is raised to 64°C, and the mixture is stirred for reaction for 4 hours;
[0059] (2) After the nano-titanium dioxide gel is dried, it is placed in a tubular furnace and calcined for 1.5 h at 930° C. to obtain modified ultrafine titanium dioxide.
[0060] The concentration of the ascorbic acid aqueous solution is 12 mg / L.
[0061] The preparation method of the sodium dioctyl sulfonate dibutyrate solution is as follows: dissolving the sodium dioctyl sulfonate dibutyrate in isooctane to obtain a 0.13 mol / L sodium dioctyl sulfonate dibutyrate solution.
[0062] The molar ratio of the template to tetrabutyl titanate is 0.4:1.
[0063] The silane coupling agent is KH560.
[0064] The drying temperature in step (2) is 55° C. and the drying time is 2.6 h.
[0065] Comparative Example 2
[0066] The difference between this comparative example and Example 1 is that the template is prepared by mixing hexadecyltrimethylammonium chloride, PEG-300 and octyltrimethylammonium bromide in a molar ratio of 1:1:1, heating to 64° C., and stirring for reaction for 4 hours.
[0067] Comparative Example 3
[0068] The difference between this comparative example and Example 1 is that the template agent is prepared by mixing hexadecyltrimethylammonium chloride and ethylene glycol in a molar ratio of 1:2.5, heating to 64°C, and stirring for reaction for 4 hours;
[0069] Comparative Example 4
[0070] The difference between this comparative example and Example 1 is that a titanate coupling agent is used for modification. The titanate coupling agent NXH-401 is purchased from Nanjing Xuanhao New Material Technology Co., Ltd.
[0071] A method for preparing modified ultrafine titanium dioxide, the preparation method comprising the following steps:
[0072] (1) 7.9 parts by volume of ethanol and 10 parts by volume of tetraethyl titanate were mixed, and the pH was adjusted to 4.3 to obtain a first mixed solution; the template was mixed with 8.1 parts by volume of ethanol, 2.3 parts by volume of water, 3 parts by volume of glacial acetic acid and 0.4 parts by volume of a titanate coupling agent to obtain a second mixed solution; the second mixed solution was slowly added dropwise to the first mixed solution to form a gel, and then aged for 9 hours to obtain a nano titanium dioxide gel;
[0073] The preparation method of the template agent is as follows: cetyl trimethyl ammonium chloride, PEG-300 and octyl trimethyl ammonium bromide in a molar ratio of 1.4:3.2:0.7 are mixed, the temperature is raised to 64°C, and the mixture is stirred for reaction for 4 hours;
[0074] (2) After the nano-titanium dioxide gel is dried, it is placed in a tube furnace at 930° C. and calcined for 1.5 h to obtain rutile nano-titanium dioxide;
[0075] (3) dispersing 100 parts by mass of rutile nano-titanium dioxide and 4 parts by mass of silver nitrate in 500 parts by mass of water, mixing them evenly to obtain a third mixed solution, mixing 1 part by volume of the third mixed solution with 13 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a first microemulsion; mixing 1 part by volume of an ascorbic acid aqueous solution with 13 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a second microemulsion; dropping the second microemulsion into the first microemulsion, stirring for 1.6 hours after the dropping is complete, to obtain a mixture;
[0076] (4) Washing the mixture, centrifuging and vacuum drying to obtain modified ultrafine titanium dioxide.
[0077] The concentration of the ascorbic acid aqueous solution is 12 mg / L.
[0078] The preparation method of the sodium dioctyl sulfonate dibutyrate solution is as follows: dissolving the sodium dioctyl sulfonate dibutyrate in isooctane to obtain a 0.13 mol / L sodium dioctyl sulfonate dibutyrate solution.
[0079] The molar ratio of the template to tetrabutyl titanate is 0.4:1.
[0080] The drying temperature in step (2) is 55° C. and the drying time is 2.6 h.
[0081] In the step (4), the mixture is washed 4 times with ethanol.
[0082] Comparative Example 5
[0083] The difference between this comparative example and Example 1 is: a preparation method of modified ultrafine titanium dioxide, the preparation method comprising the following steps:
[0084] (1) dispersing 100 parts by mass of commercially available rutile nano-titanium dioxide and 4 parts by mass of silver nitrate in 500 parts by mass of water, and mixing them uniformly to obtain a third mixed solution; mixing 1 part by volume of the third mixed solution and 13 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a first microemulsion; mixing 1 part by volume of an ascorbic acid aqueous solution and 13 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a second microemulsion; and dropping the second microemulsion into the first microemulsion, stirring for 1.6 hours after the dropping is complete, to obtain a mixture;
[0085] (2) Washing the mixture, centrifuging and vacuum drying to obtain modified ultrafine titanium dioxide.
[0086] In the step (2), the mixture is washed 4 times with ethanol.
[0087] Commercially available nano-titanium dioxide was purchased from Ningbo Jinlei Nanomaterial Technology Co., Ltd., with the product number JL-TiO2-NJ50.
[0088] Comparative Example 6
[0089] This comparative example provides a method for preparing modified ultrafine titanium dioxide, which comprises the following steps:
[0090] (1) Mix commercially available nano titanium dioxide, silane coupling agent KH560, water and ethanol in a mass ratio of 1:0.2:5:5, heat at 55 degrees Celsius for 2 hours, filter, wash and dry to obtain modified nano titanium dioxide;
[0091] (2) dispersing 100 parts by mass of modified nano-titanium dioxide and 4 parts by mass of silver nitrate in 500 parts by mass of water, mixing them evenly to obtain a third mixed solution, mixing 1 part by volume of the third mixed solution with 13 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a first microemulsion; mixing 1 part by volume of an ascorbic acid aqueous solution with 13 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a second microemulsion; dropping the second microemulsion into the first microemulsion, stirring for 1.6 hours after the dropping is complete, to obtain a mixture;
[0092] (3) Washing the mixture, centrifuging and vacuum drying to obtain modified ultrafine titanium dioxide.
[0093] In the step (3), the mixture is washed 4 times with ethanol.
[0094] Commercially available nano-titanium dioxide was purchased from Ningbo Jinlei Nanomaterial Technology Co., Ltd., with the product number JL-TiO2-NJ50.
[0095] Performance Testing
[0096] The products of Examples 1-2 and Comparative Examples 1-6 were added to commercially available ordinary glaze (composition, by mass: 10 parts of zinc oxide, 10 parts of the products of Examples 1-2 and Comparative Examples 1-6, 25 parts of transparent frit powder, 4 parts of washed soil, 0.1 part of sodium hydroxymethyl cellulose, and 0.2 part of sodium tripolyphosphate) to prepare glaze slurry, which was applied to the surface of commercially available ordinary ceramic tile bodies and fired at 1180°C to form a glaze surface to obtain ceramic tiles.
[0097] Referring to the standard JC / T897-2014 "Antibacterial Performance of Antibacterial Ceramic Products", the antibacterial rate of ceramic tiles was tested under 200-400nm ultraviolet light irradiation and 400-800nm visible light irradiation conditions.
[0098] Refer to the standard GB / T3810.4-2016 to test the strength of ceramic tiles and observe their surface cleanliness.
[0099] Table 1 Performance test results
[0100]
[0101]
[0102] The results show that the rutile nano-titanium dioxide and nano-silver prepared by the present invention synergistically exert antibacterial effects, can achieve a high antibacterial rate under ultraviolet and visible light conditions, and at the same time improve the mechanical properties of the ceramics. The nano-titanium dioxide of the present invention has a transparent glaze after being modified with a silane coupling agent, and has better dispersibility with other components, thereby improving the product quality. The glaze surface is not good when using a titanate coupling agent. Analysis shows that the product modified with a titanate coupling agent has a poor effect on improving the dispersion in the glaze.
[0103] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing modified ultrafine titanium dioxide, characterized in that: The preparation method comprises the following steps: (1) Mix 7.5-8.2 parts by volume of ethanol and 10 parts by volume of tetraethyl titanate, and adjust the pH to 4-5 to obtain a first mixed solution; mix the template with 7.5-8.2 parts by volume of ethanol, 2.1-2.4 parts by volume of water, 2.8-3.2 parts by volume of glacial acetic acid and 1.2-1.5 parts by volume of a silane coupling agent to obtain a second mixed solution; slowly dropwise add the second mixed solution to the first mixed solution, and after forming a gel, age it for 8-10 hours to obtain a nano titanium dioxide gel; The preparation method of the template agent is as follows: mixing hexadecyl trimethyl ammonium chloride, PEG-300 and octyl trimethyl ammonium bromide in a molar ratio of 1.2-1.5:3-3.5:0.6-0.9, heating to 63-65°C, and stirring for reaction for 3-5h; the molar ratio of the template agent to tetraethyl titanate is 0.3-0.5:1; the silane coupling agent is selected from one or more of silane coupling agent KH560, silane coupling agent KH550 and silane coupling agent KH570; (2) After the nano-titanium dioxide gel is dried, it is placed in a tube furnace and calcined at 900-950°C for 1-2 hours to obtain rutile nano-titanium dioxide; (3) Dispersing 100 parts by mass of rutile nano-titanium dioxide and 2-5 parts by mass of silver nitrate in 500 parts by mass of water, and mixing them evenly to obtain a third mixed solution, and mixing 1 part by volume of the third mixed solution with 12-14 parts by volume of dioctyl sodium sulfonate dibutyrate solution to obtain a first microemulsion; mixing 1 part by volume of an ascorbic acid aqueous solution with 12-14 parts by volume of a dioctyl sodium sulfonate dibutyrate solution to obtain a second microemulsion; and dropping the second microemulsion into the first microemulsion, stirring for 1-2 hours after the dropping is complete, to obtain a mixture; the concentration of the ascorbic acid aqueous solution is 10-15 mg / L; and the preparation method of the dioctyl sodium sulfonate dibutyrate solution is as follows: dissolving dioctyl sodium sulfonate dibutyrate in isooctane to obtain a 0.12-0.14 mol / L dioctyl sodium sulfonate dibutyrate solution; (4) The mixture is washed, centrifuged and vacuum dried to obtain modified ultrafine titanium dioxide.
2. The method for preparing modified ultrafine titanium dioxide according to claim 1, characterized in that: The silane coupling agent is KH560.
3. The method for preparing modified ultrafine titanium dioxide according to claim 1, characterized in that: The drying temperature in step (2) is 50-60° C. and the drying time is 2-3 hours.
4. The method for preparing modified ultrafine titanium dioxide according to claim 1, characterized in that: In the step (4), the mixture is washed 3-5 times with ethanol.
Citation Information
Patent Citations
Organic-inorganic bifunctional meso-porous titanium oxide new material and preparation method thereof
CN101538064A
Modified nano-titanium dioxide and preparation method thereof
CN104276599A
Mesoporous P25 titanium dioxide microspheres and preparation method thereof
CN107117649A
Method for producing negative ion water
CN109052749A
Noble metal carrier catalyst as well as preparation method and application thereof
CN109499566A