A kind of impermeable concrete and preparation method thereof

By using the mix ratio of SAP and polypropylene fibers in concrete, the problem of insufficient waterproofing capacity of existing anti-seepage concrete is solved, and the effect of significantly improving the anti-seepage performance and extending the service life while ensuring strength.

CN118184248BActive Publication Date: 2024-11-052ND CONSTR CO LTD OF CHINA CONSTR 5TH ENG BUREAU +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410468504.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-18
Publication Date
2024-11-05
Estimated Expiration
2044-04-18

AI Technical Summary

Technical Problem

While ensuring strength, existing impermeability-resistant concrete has limited waterproofing and permeability, and is prone to moisture penetration due to porosity and cracks, affecting the long-term stability and durability of the structure.

Method used

The mixing ratio of gravel, sand, water, gelling materials, SAP and polypropylene fiber is used to prepare concrete by mixing with a mixer, and SAP and polypropylene fiber are added to improve the structural compactness and permeability of the concrete and reduce moisture penetration.

Benefits of technology

It effectively improves the seepage resistance of concrete, extends the service life of the structure, avoids internal water loss and cracks and surface cracks, and ensures the strength and compressive resistance of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118184248B_ABST
    Figure CN118184248B_ABST
Patent Text Reader

Abstract

The present invention discloses an impermeable concrete and a preparation method thereof, belonging to the technical field of building materials. The following raw materials are selected: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 , cementitious material 325kg / m 3 , polypropylene fiber is 1‑3kg / m 3 , SAP is 0.1%-0.5% of the mass of the cementitious material. Start the mixer, add crushed stone, sand, cementitious material and water to the mixer in sequence; dilute SPA to a liquid state and stir evenly; add liquid SAP and polypropylene fiber to the mixer and stir to obtain wet concrete; pour the wet concrete into a test mold, injection mold, solidify and maintain, and obtain a concrete specimen. The preparation process of the present invention is simple, and by doubly adding SAP and polypropylene fiber and controlling their ratio, the anti-permeability performance is improved without reducing the compressive strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to an impermeable concrete and a preparation method thereof. Background Art

[0002] Water leakage in the main concrete structure of underground projects such as tunnels has always been a common quality problem. Concrete leakage will seriously affect the safety, normal use function and durability of the structure. If external moisture penetrates into the concrete, it may cause problems such as steel corrosion, concrete volume expansion, freeze-thaw damage, etc., destroy the concrete structure, and thus weaken the strength and stability of the structure; in buildings, water penetration may cause damp indoor environment, increase the risk of mold and bacteria breeding, and affect indoor air quality. Therefore, good concrete impermeability is one of the key factors to ensure the long-term stability and durability of concrete structures. At present, the impermeability of concrete has become the focus of research in the construction industry. At present, the porosity and permeation path in concrete are the main causes of permeation problems. If the density of concrete is insufficient, there are too many pores or there are permeation paths, water may pass through the concrete structure and cause permeation problems. Cracks on the surface and inside of concrete are the main channels for water penetration. Leakage is caused by cracks caused by factors such as material shrinkage, temperature changes, and loads that are not repaired in time. Impermeable concrete reduces permeation channels and improves impermeability by increasing the density of concrete and improving the pore structure. The existing impermeable concrete has high production process requirements, limited waterproof and impermeability, and low strength. In view of the above problems, the present invention provides an impermeable concrete and a preparation method thereof. Summary of the invention

[0003] The purpose of the present invention is to provide an impermeable concrete and a preparation method thereof, which can improve the impermeability of the concrete while ensuring its strength.

[0004] To achieve the above object, the present invention provides an impermeable concrete, comprising the following raw materials: crushed stone, sand, water, cementitious material, SAP and polypropylene fiber; the mix ratio of the above raw materials is: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 , cementitious material 325kg / m 3 , polypropylene fiber is 1-3kg / m 3 , SAP is 0.1%-0.5% of the mass of the cementitious material.

[0005] Preferably, the cementitious material is one or more of cement, fly ash or mineral powder.

[0006] The present invention also provides a method for preparing the above-mentioned impermeable concrete, comprising the following steps:

[0007] (1) Start the mixer and add crushed stone, sand, cementitious material and water into the mixer in sequence;

[0008] (2) Dilute the SPA into a liquid state and stir evenly;

[0009] (3) adding liquid SAP and polypropylene fiber into a mixer and stirring to obtain wet concrete;

[0010] (4) Pour the wet concrete into a test mold, perform injection molding, solidify and cure to obtain a concrete specimen.

[0011] Preferably, in step (1), the mixing time of crushed stone and sand added to the mixer is greater than 30 seconds; the mixing time after adding the cementitious material is greater than 30 seconds; and the mixing time after adding water is greater than 60 seconds.

[0012] Preferably, in step (4), the curing time is 24 hours and the curing time is 28 days.

[0013] Therefore, the present invention provides an impermeable concrete and a preparation method thereof, and the specific beneficial effects are as follows:

[0014] (1) SAP's special spatial network structure has extremely high water absorption and water retention capacity. As a high-efficiency curing agent, it can effectively avoid problems such as water loss and cracking caused by internal hydration of concrete;

[0015] (2) Adding polypropylene fibers to concrete can improve its internal structure, fill pores, and effectively prevent concrete segregation and bleeding, thereby inhibiting the shrinkage of large-volume concrete during the plastic process and preventing cracks on its surface;

[0016] (3) The present invention achieves the goal of improving the anti-seepage performance while ensuring the strength of concrete, reducing water penetration, and extending the service life of the concrete structure by adding SAP and polypropylene fibers to concrete and designing a certain mix ratio.

[0017] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a trend diagram of the impact on the anti-permeability performance of concrete prepared in the embodiment of the present invention and the comparative example;

[0019] Figure 2 It is a trend diagram of the compressive properties of concrete prepared in the embodiments of the present invention and the comparative examples. DETAILED DESCRIPTION

[0020] The present invention provides an impermeable concrete, comprising the following raw materials in the following mix ratios: crushed stone 1175 kg / m 3、Sand 720kg / m 3 , water 180kg / m 3 , cementitious material 325kg / m 3 , polypropylene fiber is 1-3kg / m 3 , SAP is 0.1%-0.5% of the mass of the cementitious material.

[0021] Wherein, the cementitious material is one or more of cement, fly ash or mineral powder.

[0022] The present invention also provides a method for preparing the above-mentioned impermeable concrete, comprising the following steps:

[0023] (1) Start the mixer, first add crushed stone and sand into the mixer and stir for more than 30 seconds, then add cementitious material and stir for more than 30 seconds, and finally add water and stir for more than 60 seconds;

[0024] (2) Dilute the SPA into a liquid state and stir evenly;

[0025] (3) adding liquid SAP and polypropylene fiber into a mixer and stirring to obtain wet concrete;

[0026] (4) Pour the wet concrete into the test mold, inject and cure for 24 hours, and then cure for 28 days to obtain the concrete specimen.

[0027] The following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] This embodiment provides an anti-seepage concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3 , add 0.1% SAP of the mass ratio of the cementitious material, and add 1kg / m 3 Polypropylene fibers are used to prepare concrete.

[0030] The method for preparing the above-mentioned impermeable concrete specifically comprises the following steps:

[0031] (1) Start the mixer, first add crushed stone and sand into the mixer and stir for more than 30 seconds, then add cement, fly ash and mineral powder and stir for more than 30 seconds, and finally add water and stir for more than 60 seconds;

[0032] (2) Dilute the SPA into a liquid state and stir evenly;

[0033] (3) adding liquid SAP and polypropylene fiber into a mixer and stirring to obtain wet concrete;

[0034] (4) Pour the wet concrete into the test mold, inject and cure for 24 hours, and then cure for 28 days to obtain the concrete specimen.

[0035] Example 2

[0036] This embodiment provides an anti-seepage concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3 , add 0.3% SAP of the mass ratio of the cementitious material, and add 1kg / m 3 Polypropylene fibers are used to prepare concrete.

[0037] The method for preparing concrete in this embodiment is the same as that in Embodiment 1, and will not be repeated here.

[0038] Example 3

[0039] This embodiment provides an anti-seepage concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3 , add 0.5% SAP of the mass ratio of the cementitious material, and add 1kg / m 3 Polypropylene fibers are used to prepare concrete.

[0040] The method for preparing concrete in this embodiment is the same as that in Embodiment 1, and will not be repeated here.

[0041] Example 4

[0042] This embodiment provides an anti-seepage concrete, which is made of the following raw materials: crushed stone 1175kg / m3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3 , add 0.1% SAP of the mass ratio of the cementitious material, and add 2kg / m 3 Polypropylene fibers are used to prepare concrete.

[0043] The method for preparing concrete in this embodiment is the same as that in Embodiment 1, and will not be repeated here.

[0044] Example 5

[0045] This embodiment provides an anti-seepage concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3 , add 0.3% SAP of the mass ratio of the cementitious material, and add 2kg / m 3 Polypropylene fibers are used to prepare concrete.

[0046] The method for preparing concrete in this embodiment is the same as that in Embodiment 1, and will not be repeated here.

[0047] Example 6

[0048] This embodiment provides an anti-seepage concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3 , add 0.5% SAP of the mass ratio of the cementitious material, and add 2kg / m 3 Polypropylene fibers are used to prepare concrete.

[0049] The method for preparing concrete in this embodiment is the same as that in Embodiment 1, and will not be repeated here.

[0050] Example 7

[0051] This embodiment provides an anti-seepage concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3 , add 0.1% SAP of the mass ratio of the cementitious material, and add 3kg / m 3 Polypropylene fibers are used to prepare concrete.

[0052] The method for preparing concrete in this embodiment is the same as that in Embodiment 1, and will not be repeated here.

[0053] Example 8

[0054] This embodiment provides an anti-seepage concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3 , add 0.3% SAP of the mass ratio of the cementitious material, and add 3kg / m 3 Polypropylene fibers are used to prepare concrete.

[0055] The method for preparing concrete in this embodiment is the same as that in Embodiment 1, and will not be repeated here.

[0056] Example 9

[0057] This embodiment provides an anti-seepage concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3 , add 0.5% SAP of the mass ratio of the cementitious material, and add 3kg / m 3 Polypropylene fibers are used to prepare concrete.

[0058] The method for preparing concrete in this embodiment is the same as that in Embodiment 1, and will not be repeated here.

[0059] Comparative Example 1

[0060] This comparative example provides a concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 , cement 325kg / m 3 , to prepare concrete.

[0061] The method for preparing the concrete specifically comprises the following steps:

[0062] (1) Start the mixer, first add crushed stone and sand into the mixer and stir for more than 30 seconds, then add cement and stir for more than 30 seconds, and finally add water and stir for more than 60 seconds to obtain wet concrete;

[0063] (2) Pour the wet concrete into the test mold, inject and cure for 24 hours, and then cure for 28 days to obtain the concrete specimen.

[0064] Comparative Example 2

[0065] This comparative example provides a concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3 , to prepare concrete.

[0066] The method for preparing the concrete specifically comprises the following steps:

[0067] (1) Start the mixer, first add crushed stone and sand into the mixer and stir for more than 30 seconds, then add cement, fly ash and mineral powder and stir for more than 30 seconds, and finally add water and stir for more than 60 seconds;

[0068] (2) Pour the wet concrete into the test mold, inject and cure for 24 hours, and then cure for 28 days to obtain the concrete specimen.

[0069] Comparative Example 3

[0070] This comparative example provides a concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3, SAP with a mass ratio of 0.1% of cementitious material was added to prepare concrete.

[0071] The method for preparing the concrete specifically comprises the following steps:

[0072] (1) Start the mixer, first add crushed stone and sand into the mixer and stir for more than 30 seconds, then add cement, fly ash and mineral powder and stir for more than 30 seconds, and finally add water and stir for more than 60 seconds;

[0073] (2) Dilute the SPA into a liquid state and stir evenly;

[0074] (3) adding liquid SAP into a mixer and mixing to obtain wet concrete;

[0075] (4) Pour the wet concrete into the test mold, inject and cure for 24 hours, and then cure for 28 days to obtain the concrete specimen.

[0076] Comparative Example 4

[0077] This comparative example provides a concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3 , SAP with a mass ratio of 0.3% of cementitious material was added to prepare concrete.

[0078] The preparation method of the concrete in this comparative example is the same as that in comparative example 3, and will not be repeated here.

[0079] Comparative Example 5

[0080] This comparative example provides a concrete, which is made of the following raw materials: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 、Cement 276.88kg / m 3 、Fly ash 32.46kg / m 3 、Mineral powder 16.23kg / m 3 , SAP with a mass ratio of 0.5% of cementitious material was added to prepare concrete.

[0081] The preparation method of the concrete in this comparative example is the same as that in comparative example 3, and will not be repeated here.

[0082] The concrete specimens obtained above were tested for compression and impermeability. The test results are shown in Table 1 and Figure 1-2 shown.

[0083]

[0084]

[0085] The failure mode of concrete mixed with SAP and polypropylene fiber shows a certain plasticity. After the specimen is damaged by compression, it will not collapse. Only a few fragments are squeezed and fall off. The rest of the parts have strong integrity and good compressive performance. Adding an appropriate amount of SAP and polypropylene fiber will effectively improve the anti-permeability of concrete, while excessive addition will reduce its anti-permeability.

[0086] From the data in the table and Figure 1 and Figure 2 It can be seen that the addition of SAP alone can change the compressive failure morphology of concrete from brittle failure to plastic failure. When SAP accounting for 0.1%-0.3% of the mass of cementitious materials is added, there is almost no adverse effect on the compressive performance of concrete, but when excessive SAP is added (such as 0.5% of the mass of cementitious materials), it will have a serious adverse effect on the compressive performance of concrete, and the minimum compressive strength will drop to 26.57MPa, a decrease of 13.54% compared with the same period last year.

[0087] The double addition of SAP and polypropylene fiber can change the compressive failure mode of concrete from brittle failure to plastic failure, which is a feature that single addition of SAP does not have. The appropriate amount of double addition of SAP (0.1%) and polypropylene fiber (no more than 2kg / m 3 ), it has almost no adverse effect on the compressive strength of concrete, and may even slightly improve it; but when the SAP content is too large (0.5%), its compressive strength will be greatly reduced, and the minimum will drop to 23.83MPa, which is 22.39% lower than the previous strength.

[0088] Appropriate amount of double-doped SAP (0.1%) and polypropylene fiber (1kg / m 3 ), will effectively improve the anti-penetration ability of concrete, and the minimum water seepage height can be reduced to 92.2mm, which is 18.84% lower than before; excessive addition of SAP (0.5%) or polypropylene fiber (3kg / m 3 ), will cause its anti-penetration ability to be greatly reduced, and the water seepage height can rise to 146.1mm at most, an increase of 28.61% compared with before.

[0089] Compared with the comparative example 2 in Table 1 (compressive strength 30.73MPa, water seepage height 113.6mm), the appropriate amount of SAP (between 0.1% and 0.3%) and polypropylene fiber (0-2kg / m 3 ), the concrete can improve its impermeability without almost reducing its compressive strength.

[0090] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. An impermeable concrete, It is characterized in that It is composed of the following raw materials: crushed stone, sand, water, cementitious material, SAP and polypropylene fiber; the proportion of the above raw materials is: crushed stone 1175kg / m 3 、Sand 720kg / m 3 , water 180kg / m 3 , cementitious material 325kg / m 3 , polypropylene fiber is 1-3kg / m 3 , SAP is 0.1%-0.5% of the mass of the cementitious material; The cementitious materials are cement, fly ash and mineral powder.

2. A method for preparing an impermeable concrete according to claim 1, It is characterized in that The following steps are involved: (1) Start the mixer and add crushed stone, sand, cementitious material and water into the mixer in sequence; (2) Dilute the SPA into a liquid state and stir evenly; (3) adding liquid SAP and polypropylene fiber into a mixer and mixing to obtain wet concrete; (4) Pour the wet concrete into the test mold, inject and solidify it, and then cure it to obtain a concrete specimen.

3. A method for preparing an impermeable concrete according to claim 2, It is characterized in that In step (1), the crushed stone and sand are added to the mixer and stirred for more than 30 seconds; the cementitious material is added and stirred for more than 30 seconds; and the water is added and stirred for more than 60 seconds.

4. A method for preparing an impermeable concrete according to claim 2, It is characterized in that In step (4), the curing time is 24 hours and the curing time is 28 days.

Citation Information

Cited By

  • Impermeable concrete and preparation method thereof

    CN119750994A