A heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microsphere and its preparation method and application
By preparing heat-resistant, swelling-resistant, electrochemically active, and stable cross-linked polymer microspheres, the problem of poor stability of lithium-ion battery separators at high temperatures was solved, achieving low-cost, high-performance battery separator improvement.
Patent Information
- Application Number
- CN202410400979.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-03
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-04-03
AI Technical Summary
Existing lithium-ion battery separators have poor stability at high temperatures, posing an explosion risk, and inorganic powder materials are expensive.
A heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microspheres were prepared by emulsification polymerization using a combination of oil-soluble and water-soluble nonionic surfactants. The microspheres have controllable size and possess excellent electronic insulation, thermal stability, and affinity for electrolytes.
The prepared microspheres exhibit good thermal stability, resistance to electrolyte swelling, low cost, appropriate porosity, and coating stability, thereby improving the safety and performance of lithium-ion batteries.
Smart Images

Figure CN118184868B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer microsphere material preparation, and in particular to heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microspheres and a preparation method and application thereof. Background Art
[0002] The battery separator plays the role of separating the positive and negative electrodes in the battery system, blocking the passage of electrons in the circuit during charging and discharging, and allowing the free passage of lithium ions in the electrolyte. It can selectively close the micropores when the battery is charging and discharging or when the temperature rises to limit excessive current and prevent short circuits. The quality of its performance directly determines the overall performance of the battery.
[0003] The current mainstream directions include multi-layer composite membranes, which are PP / PE two-layer composite membranes or PP / PE / PP three-layer composite membranes independently developed by Celgard Corporation of the United States. They combine the advantages of PP membrane's good mechanical properties and high melting temperature with PE membrane's softness, good toughness and low closed-cell temperature, thereby increasing the safety performance of the battery. However, PE and PP membranes have poor affinity for electrolytes, and the fiber structure of the PP / PE / PP three-layer membrane is linear. Once a short circuit occurs, the short circuit area will expand rapidly in an instant, the heat will rise sharply and be difficult to discharge, and there is a potential for explosion.
[0004] Traditional lithium-ion battery separators have low melting points (PE is 135°C, PP is 165°C), and poor stability at high temperatures, which seriously affects the safety of the battery. It is necessary to improve its thermodynamic stability to meet the higher requirements of lithium batteries. At present, inorganic powders with high heat resistance and mechanical strength (such as alumina Al2O3, boehmite AlOOH, etc.) are used to prepare lithium battery ceramic composite separators, which can improve the mechanical strength of the separator and reduce the thermal shrinkage of the separator.
[0005] ES CHOI et al. dip-coated ceramic particles on both sides of a PET non-woven film with good heat resistance, which increased the conductivity of the film by 50% compared with the traditional PE film. Hitachi Maxell of Japan coated plate-shaped inorganic particles on the surface of the base film to maintain the integrity of the shape at high temperatures. However, the high-purity, high-uniformity submicron inorganic material particles used in the above-mentioned prior art are expensive and not cost-effective. Summary of the invention
[0006] The purpose of the present invention is to overcome at least one of the defects of the above-mentioned prior art and to provide a heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microsphere and its preparation method and application. The microsphere has excellent electronic insulation; controllable size and good uniformity; resistance to swelling or corrosion by electrolyte; good thermal stability; good affinity with electrolyte and a certain liquid absorption rate; good coating stability and flatness, and appropriate porosity.
[0007] The purpose of the present invention can be achieved by the following technical solutions:
[0008] One of the purposes of the present invention is to provide a method for preparing heat-resistant and swelling-resistant electrochemically active stable cross-linked polymer microspheres, comprising the following steps:
[0009] The oil-soluble nonionic surfactant and the water-soluble nonionic surfactant are mixed to obtain a compound nonionic surfactant;
[0010] Mixing monomer A, monomer B and monomer C to obtain a mixed monomer;
[0011] Adding a compounded nonionic surfactant to the mixed monomer, and then adding water, shearing and emulsifying to obtain a mixed monomer emulsion;
[0012] A portion of the mixed monomer emulsion is put into a reactor and an initiator is added to react in an inert atmosphere at a reaction temperature of 60 to 95°C. The remaining mixed monomer emulsion is dropwise added to the reactor during the reaction. After the dropwise addition is complete, the reaction temperature is further increased to 65 to 100°C. After the reaction is sufficient, the mixture is filtered, washed, and dried to obtain heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microspheres.
[0013] Furthermore, the mass ratio of the mixed monomer to the compounded nonionic surfactant is 2500:1 to 10:1.
[0014] Furthermore, the mass ratio of the oil-soluble nonionic surfactant to the water-soluble nonionic surfactant is 99:1 to 1:3.
[0015] Furthermore, the oil-soluble nonionic surfactant includes but is not limited to one or more of AEO20, AEO40, AEO60, AEO80, AEO7, AEO9, AEO11, AEO12, AEO13, AEO14, AEO15, AEO20, and AEO23; the water-soluble nonionic surfactant includes but is not limited to one or more of Tween 20, Tween 21, Tween 40, Tween 60, Tween 61, Tween 80, Tween 81, Tween 85, AEO3, AEO4, and AEO5.
[0016] Furthermore, the mass proportion of the monomer A in the mixed monomer is 3-90%; the mass proportion of the monomer B in the mixed monomer is 5-90%; and the mass proportion of the monomer C in the mixed monomer is 1-50%.
[0017] Further:
[0018] The monomer A is selected from the group consisting of, but not limited to, styrene, ethylene, vinyl acetate, vinyl chloride, vinylidene chloride, chloromethylstyrene, acrylamide, acrylonitrile, 2-methyl-5-vinylpyridine, sodium p-vinylbenzenesulfonate, N-vinylformamide, N-vinylpyrrolidone, and aniline;
[0019] The monomer B includes, but is not limited to, one or more of acrylic acid, methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, lauryl acrylate, glycidyl acrylate, methacrylic acid, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, glycidyl methacrylate, allyl glycidyl ether, adipic dihydrazide, carbonate dihydrazide, oxalic acid dihydrazide, succinic acid dihydrazide, N-aminoacrylamide, methylenebisacrylamide, itaconic acid, maleic acid, maleic anhydride or fumaric acid;
[0020] The monomer C includes, but is not limited to, one or more of divinylbenzene, butadiene, isoprene, 2,3-dimethylbutadiene, 1,3-pentadiene, chloroprene, ethylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropyl triacrylate, ethoxytrimethylolpropane triacrylate, diallyl maleate, allyl methacrylate, pentaerythritol triallyl ether, pentaerythritol diacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, diallyl terephthalate, N-hydroxymethyl acrylamide, N-methoxymethyl acrylamide, N-isopropyloxymethyl acrylamide, N-butoxymethyl acrylamide, N-isobutyloxymethyl acrylamide, N-octyloxymethyl acrylamide, or N-carboxymethyloxymethyl acrylamide.
[0021] Furthermore, the initiator includes, but is not limited to, one or more of ammonium persulfate, potassium persulfate, sodium persulfate, hydrogen peroxide, tert-butyl hydroperoxide, benzoyl peroxide, azobisisobutyronitrile or cumene hydroperoxide.
[0022] The second object of the present invention is to provide a heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microsphere, which is prepared by the preparation method as described above, and the microsphere size is 100nm-10μm, and the thermal decomposition temperature of the microsphere is 250-430℃.
[0023] The third object of the present invention is to use the heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microspheres as a coating in a lithium-ion battery separator.
[0024] Compared with the prior art, the present invention provides a heat-resistant and swelling-resistant electrochemically active stable cross-linked polymer microsphere, which has excellent electronic insulation. Thanks to the advantages of emulsion polymerization, the obtained microspheres are controllable in size and have good uniformity. Thanks to the cross-linking effect of monomer C, the microspheres are resistant to swelling or corrosion of the electrolyte. Thanks to the heat resistance of monomer A, the obtained microspheres have good thermal stability. Thanks to the compounding of surfactants, the microsphere surface has good affinity with the electrolyte and has a certain liquid absorption rate. It also has the advantages of appropriate porosity, good coating stability and flatness, low cost, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1A This is a scanning electron microscope photo of the microspheres prepared in Example 1;
[0026] Figure 1B This is a scanning electron microscope photo of the microspheres prepared in Example 2;
[0027] Figure 1C This is a scanning electron microscope photo of the microspheres prepared in Example 3;
[0028] Figure 1D This is a scanning electron microscope photo of the microspheres prepared in Comparative Example 4;
[0029] Figure 2A This is a scanning electron microscope photograph of the microspheres prepared in Example 1 after being immersed in a lithium battery electrolyte at 85°C for 24 hours;
[0030] Figure 2B This is a scanning electron microscope photograph of the microspheres prepared in Example 2 after being immersed in a lithium battery electrolyte at 85°C for 24 hours;
[0031] Figure 2C This is a scanning electron microscope photograph of the microspheres prepared in Example 3 after being immersed in a lithium battery electrolyte at 85°C for 24 hours;
[0032] Figure 2D This is a scanning electron microscope photo of the microspheres prepared in Comparative Example 4 after being immersed in a lithium battery electrolyte at 85°C for 24 hours;
[0033] Figure 3A is the thermogravimetric (TGA) curve of the microspheres prepared in Example 1;
[0034] Figure 3B This is the thermogravimetric (TGA) curve of the microspheres prepared in Comparative Example 4. DETAILED DESCRIPTION
[0035] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0036] Example 1
[0037] The raw materials and their proportions are shown in the table below:
[0038]
[0039] 1. Emulsification: According to the above table, Tween 80 and Span 80 are measured and mixed evenly to obtain a compound nonionic surfactant; according to the above table, dipentaerythritol hexaacrylate, styrene, methyl methacrylate and acrylonitrile are weighed and mixed evenly to obtain a mixed monomer; the compound nonionic surfactant is added to the mixed monomer, and then 400 ml of deionized water is added, and shearing is performed for emulsification to obtain a mixed monomer emulsion.
[0040] 2. Feeding: Add 2280 ml of deionized water into the reactor (10 L), start stirring at a rate of 170 rpm. After nitrogen is introduced for 0.5 h, add 3 / 10 of the mixed monomer emulsion and stir mechanically for 2.5 h.
[0041] 3. Polymerization reaction: raise the temperature to 67°C, weigh 6 g of potassium persulfate and dissolve it in 120 mL of water, then put it into the reactor and reduce the speed to 80 rpm.
[0042] 4. Dropwise addition: 1.5 hours after the start of polymerization, add the remaining emulsion dropwise for 4 hours.
[0043] 5. Heating: 16 hours after the start of polymerization, raise the temperature to 84°C.
[0044] 6. Discharging: 20 hours after the start of polymerization, discharging, filter pressing and drying, the heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microspheres are obtained. The average size of the microspheres is about 200nm, and the thermal decomposition temperature is 361℃. Figure 1A , Figure 3A .
[0045] The microspheres obtained in this example were immersed in a lithium battery electrolyte at 85°C for 24 hours, and it was found that the particle size did not change substantially, indicating that the microspheres were resistant to swelling or corrosion by the electrolyte. Figure 2A .
[0046] Example 2
[0047] The raw materials and their proportions are shown in the table below:
[0048]
[0049]
[0050] 1. Emulsification: According to the above table, Tween 80 and Span 80 are measured and mixed evenly to obtain a compound nonionic surfactant; according to the above table, dipentaerythritol hexaacrylate, styrene, methyl methacrylate and acrylonitrile are weighed and mixed evenly to obtain a mixed monomer; the compound nonionic surfactant is added to the mixed monomer, and then 400 ml of deionized water is added, and shearing is performed for emulsification to obtain a mixed monomer emulsion.
[0051] 2. Feeding: Add 2280 ml of deionized water into the reactor (10 L), start stirring at a rate of 170 rpm. After nitrogen is introduced for 0.5 h, add 3 / 10 of the mixed monomer emulsion and stir mechanically for 2.5 h.
[0052] 3. Polymerization reaction: raise the temperature to 67°C, weigh 6 g of potassium persulfate and dissolve it in 120 mL of water, then put it into the reactor and reduce the speed to 80 rpm.
[0053] 4. Dropwise addition: 1.5 hours after the start of polymerization, add the remaining mixed monomer emulsion dropwise for 4 hours.
[0054] 5. Heating: 16 hours after the start of polymerization, raise the temperature to 84°C.
[0055] 6. Discharging: 20 hours after the start of polymerization, discharging, filter pressing and drying, to obtain heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microspheres. The average size of the microspheres is about 370nm. Figure 1B , the thermal decomposition temperature is 350℃.
[0056] The microspheres obtained in this example were immersed in a lithium battery electrolyte at 85°C for 24 hours, and it was found that the particle size did not change substantially, indicating that the microspheres were resistant to swelling or corrosion by the electrolyte. Figure 2B .
[0057] Example 3
[0058] The raw materials and their proportions are shown in the table below:
[0059]
[0060] 1. Emulsification: According to the above table, Tween 80 and Span 80 are measured and mixed evenly to obtain a compound nonionic surfactant; according to the above table, dipentaerythritol hexaacrylate, styrene, methyl methacrylate and acrylonitrile are weighed and mixed evenly to obtain a mixed monomer; the compound nonionic surfactant is added to the mixed monomer, and then 400 ml of deionized water is added, and shearing is performed for emulsification to obtain a mixed monomer emulsion.
[0061] 2. Feeding: Add 2400 ml of deionized water into the reactor (10 L), start stirring at a rate of 170 rpm. After nitrogen is introduced for 0.5 h, add 3 / 10 of the mixed monomer emulsion and mechanically stir for 2.5 h.
[0062] 3. Polymerization reaction: raise the temperature to 67°C, weigh 6 g of potassium persulfate and dissolve it in 120 mL of water, then put it into the reactor and reduce the speed to 80 rpm.
[0063] 4. Dropwise addition: 1.5 hours after the start of polymerization, add the remaining mixed monomer emulsion dropwise for 4 hours.
[0064] 5. Heating: 16 hours after the start of polymerization, raise the temperature to 84°C.
[0065] 6. Discharging: 20 hours after the start of polymerization, discharging, filter pressing and drying, to obtain heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microspheres. The average size of the microspheres is about 450nm. Figure 1C , thermal decomposition temperature 360℃.
[0066] The microspheres obtained in this example were immersed in a lithium battery electrolyte at 85°C for 24 hours, and it was found that the particle size did not change substantially, indicating that the microspheres were resistant to swelling or corrosion by the electrolyte. Figure 2C .
[0067] Comparative Example 1
[0068] The raw materials and their proportions are shown in the table below:
[0069]
[0070] The preparation process of this comparative example is basically the same as that of Example 2, except that in this comparative example, the amount of the oil-soluble nonionic surfactant is 6.3 ml, and the amount of the water-soluble nonionic surfactant is 0.
[0071] Since the comparative example used a pure oil-soluble surfactant during the preparation process, after the reaction was completed within the same time, the monomer smell of the reaction liquid was strong, which meant that the toxic monomer conversion was incomplete and subsequent processing was required, which had an adverse impact on personnel safety and production.
[0072] Comparative Example 2
[0073] The raw materials and their proportions are shown in the table below:
[0074]
[0075] The preparation process of this comparative example is basically the same as that of Example 2, except that in this comparative example, the amount of oil-soluble nonionic surfactant is 0 and the amount of water-soluble nonionic surfactant is 6.3 ml.
[0076] Since a pure water-soluble surfactant was used in the preparation process of this comparative example, a large amount of agglomerates were generated after the reaction was completed within the same time, and phase separation occurred, and no qualified product could be obtained.
[0077] Comparative Example 3
[0078] The raw materials and their proportions are shown in the table below:
[0079]
[0080] The preparation process of this comparative example is basically the same as that of Example 1, and the average size of the obtained microspheres is about 500nm. Figure 1D The difference is that only monomer A is used in this comparative example, and monomer B or monomer C is not used, resulting in poor swelling resistance of the microspheres, and partial swelling and dissolution occurred in the lithium battery electrolyte, such as Figure 2D shown.
[0081] Comparative Example 4
[0082] The raw materials and their proportions are shown in the table below:
[0083]
[0084] The preparation process of this comparative example is basically the same as that of Example 1, except that only monomer B is used in this comparative example, and monomer A or monomer C is not used, resulting in poor thermal stability of the microspheres, which begin to decompose at 255°C. Figure 3B shown.
[0085] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. Application of heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microspheres as a coating in lithium-ion battery separators, characterized in that: The preparation of the polymer microspheres comprises the following steps: The oil-soluble nonionic surfactant and the water-soluble nonionic surfactant are mixed to obtain a compound nonionic surfactant; Mixing monomer A, monomer B and monomer C to obtain a mixed monomer; Adding a compounded nonionic surfactant to the mixed monomer, and then adding water, shearing and emulsifying to obtain a mixed monomer emulsion; A portion of the mixed monomer emulsion is put into a reactor and an initiator is added to react in an inert atmosphere at a reaction temperature of 60-95°C. The remaining mixed monomer emulsion is added dropwise to the reactor during the reaction. After the addition is complete, the reaction temperature is further increased to 65-100°C. After the reaction is sufficient, the mixture is filtered, washed, and dried to obtain heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microspheres. The monomer A is selected from one or more of styrene, ethylene, vinyl acetate, vinyl chloride, vinylidene chloride, chloromethylstyrene, acrylamide, acrylonitrile, 2-methyl-5-vinylpyridine, sodium p-vinylbenzenesulfonate, N-vinylformamide, N-vinylpyrrolidone or aniline; The monomer B is selected from one or more of acrylic acid, methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, lauryl acrylate, glycidyl acrylate, methacrylic acid, methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, glycidyl methacrylate, allyl glycidyl ether, adipic dihydrazide, carbonate dihydrazide, oxalic acid dihydrazide, succinic acid dihydrazide, N-aminoacrylamide, methylenebisacrylamide, itaconic acid, maleic acid, maleic anhydride or fumaric acid; The monomer C is selected from one or more of divinylbenzene, butadiene, isoprene, 2,3-dimethylbutadiene, 1,3-pentadiene, chloroprene, ethylene glycol diacrylate, triethylene glycol diacrylate, polyethylene glycol diacrylate, tripropylene glycol diacrylate, trimethylolpropyl triacrylate, ethoxylated trimethylolpropane triacrylate, diallyl maleate, allyl methacrylate, pentaerythritol triallyl ether, pentaerythritol diacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, diallyl terephthalate, N-hydroxymethyl acrylamide, N-methoxymethyl acrylamide, N-isopropyloxymethyl acrylamide, N-butoxymethyl acrylamide, N-isobutyloxymethyl acrylamide, N-octyloxymethyl acrylamide or N-carboxymethyloxymethyl acrylamide; The mass ratio of the mixed monomer to the compounded nonionic surfactant is 2500:1~10:1; The oil-soluble nonionic surfactant is selected from one or more of Sban 20, Sban 40, Sban 60, Sban 80, AEO7, AEO9, AEO11, AEO12, AEO13, AEO14, AEO15, AEO20, and AEO23; The water-soluble nonionic surfactant is selected from one or more of Tween 20, Tween 21, Tween 40, Tween 60, Tween 61, Tween 80, Tween 81, Tween 85, AEO3, AEO4, and AEO5; The mass proportion of the monomer A in the mixed monomer is 3-90%; The mass proportion of the monomer B in the mixed monomer is 5-90%; The mass proportion of the monomer C in the mixed monomer is 1-50%.
2. The use of a heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microsphere as a coating in a lithium-ion battery separator according to claim 1, characterized in that: The mass ratio of the oil-soluble nonionic surfactant to the water-soluble nonionic surfactant is 99:1 to 1:
3.
3. The use of the heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microspheres as a coating in a lithium-ion battery separator according to claim 1, characterized in that: The initiator is selected from one or more of ammonium persulfate, potassium persulfate, sodium persulfate, hydrogen peroxide, tert-butyl hydroperoxide, benzoyl peroxide, azobisisobutyronitrile or cumene hydroperoxide.
4. The use of the heat-resistant, swelling-resistant, electrochemically active, stable cross-linked polymer microspheres as a coating in a lithium-ion battery separator according to claim 1, characterized in that: The size of the microspheres prepared by the preparation method is 100 nm-10 μm, and the thermal decomposition temperature of the microspheres is 250-430°C.