A low-temperature adhesive and a preparation method thereof, and a corrugated paper production process containing the low-temperature adhesive

Through the combination of low-temperature adhesives, the use of raw materials such as denatured starch and low-temperature resin glue, the problems of insufficient bonding power of corrugated carton adhesive and high energy consumption are solved, and the stable bonding and low-energy production of corrugated paper are achieved.

CN118185509BActive Publication Date: 2024-11-22DONGGUAN RUIFENG PAPER PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410402966.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-03
Publication Date
2024-11-22
Estimated Expiration
2044-04-03

AI Technical Summary

Technical Problem

The adhesive bonding power of existing corrugated cartons is weak, has poor compressive resistance, mildew resistance, corrosion resistance and moisture resistance, and has high energy consumption and difficult temperature control during processing in low-temperature environments, resulting in unstable bonding and cracking.

Method used

Low-temperature adhesive consists of denatured starch, low-temperature resin glue and borax, combined with water-soluble resin, amino resin and nano zinc oxide and other raw materials to form adhesives with better adhesion, low-temperature resistance and film formation properties, for use in Low temperature bonding of corrugated paper.

Benefits of technology

The stable bonding of corrugated paper is achieved at lower temperatures, reducing shedding and cracking, reducing production energy consumption, and improving production efficiency and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present application relates to a low-temperature adhesive, which is composed of the following raw materials in parts by weight: 25-38 parts of modified starch, 2-3 parts of low-temperature resin glue, 0.3-0.5 parts of borax, and 135-150 parts of water. Corrugated paper is made by the following method: the first base paper is thermoformed to form a corrugated structure, the surface of the second base paper is sprayed with a low-temperature adhesive, and the side containing the adhesive is transferred to the surface of a base paper for bonding, and the thermal bonding is stabilized by a bonding device to form a semi-finished product; the side of the adhesive surface of the second base paper raw material of the semi-finished product is coated with a low-temperature adhesive, and the adhesive surface of the obtained second base paper is transferred to the surface of the third base paper for bonding, and then hot pressing and shearing are performed to obtain corrugated paper. It can be thermally bonded at a lower temperature. Therefore, when producing corrugated paper in winter, at its relatively low processing temperature, the temperature can be better controlled, while reducing energy consumption, so that the corrugated paper layer structure is bonded and stable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of corrugated paper, and more specifically, to a low-temperature adhesive and a preparation method thereof, and a corrugated paper production process containing the adhesive. Background Art

[0002] Corrugated paperboard is widely used in the packaging box industry due to its excellent strength and plasticity. Corrugated paperboard is a paper composite board, a non-metallic sandwich material with viscoelastic plasticity, which is made of corrugated corrugated core paper and inner and outer surface papers. The basic structure of corrugated paperboard is explained by taking single corrugated paperboard as an example. Single corrugated paperboard, that is, three-layer corrugated paperboard, is made of surface paper, inner paper and a layer of corrugated core paper. Adhesive is an indispensable material for corrugated paperboard manufacturers. At present, starch glue is mainly used for bonding corrugated paperboard. However, due to the weak bonding force of this type of adhesive, poor compression resistance, mildew resistance, corrosion resistance and moisture resistance, the quality of the products produced cannot be guaranteed.

[0003] Therefore, some technologies add phenolic resin, EAA emulsion and other resin glues with higher film-forming temperature to starch glue to improve its adhesion, mildew resistance, moisture resistance, and water resistance. However, the addition of the above resin glues may also lead to an increase in the bonding temperature, bonding time, and bonding pressure of corrugated cardboard during the processing process, thereby increasing energy consumption in the production process, which is not conducive to production.

[0004] Since the corrugated paper production process is highly automated, when the indoor temperature is low in winter, a large amount of energy is consumed during the processing to maintain a high bonding temperature. The energy loss is large, and the bonding temperature is difficult to control. As a result, when the corrugated paper is processed and bonded, it is easy for the temperature in some positions to fail to reach the curing temperature, which in turn leads to unstable bonding in some positions, reducing the stability of the layer structure of the corrugated paper, and causing the corrugated paper to crack during use. Therefore, it is necessary to study a low-temperature adhesive. Summary of the invention

[0005] In order to obtain better adhesion and enable corrugated paper lamination processes to be performed at lower temperatures, the present application provides a low-temperature adhesive and a preparation method and a corrugated paper production process containing the adhesive.

[0006] In a first aspect, the present application provides a low-temperature adhesive, which is composed of the following raw materials in parts by weight:

[0007] Modified starch 25-38 parts

[0008] 2-3 parts of low temperature resin glue

[0009] Borax 0.3-0.5 parts

[0010] 135-150 parts of water.

[0011] The dosage of the above raw materials is the best choice for this application. Among them, modified starch is soluble in water. Modified starch has low gelatinization temperature, high transparency, high solubility, strong gelling property, good freeze-thaw stability, and low temperature resistance. It also has the advantages of film-forming property, water retention, adhesive property, non-toxicity, tastelessness, biocompatibility, thixotropy, etc. Therefore, using modified starch as the main raw material of adhesive has better environmental protection and better low temperature resistance.

[0012] Low-temperature resin glue is an adhesive with the advantages of low-temperature resistance, adhesion, and film-forming properties. It can quickly solidify in a relatively low temperature environment, making the bonding of carton boards stable.

[0013] The film-forming temperature of the low-temperature adhesive of the present application is 90-118° C., and within this temperature range, it is difficult for the adhesive to which the phenolic resin is added to form a complete film, thus resulting in lower bonding strength and the like.

[0014] The low temperature in the present application refers to a low film-forming temperature, which is lower than the film-forming temperature of commercially available phenolic resin-modified starch glue. Therefore, during the production process, energy consumption is low, production efficiency is high, and cost is low.

[0015] Borax has a water-absorbing effect, which further promotes the film formation of low-temperature adhesives and shortens the curing time.

[0016] Therefore, the present application adopts low-temperature resin glue and modified starch for compounding, and under the action of water and borax, the obtained low-temperature resin adhesive has better adhesion, adhesion, low-temperature resistance, etc. Therefore, when used in the production of corrugated paper, it can be adhered and bonded at a lower temperature, so that the layer structure of the corrugated paper is bonded stably and the possibility of falling off is reduced.

[0017] Preferably, the low-temperature resin glue is composed of the following raw materials in percentage by weight:

[0018] Water-soluble resin 15-23%

[0019] Amino resin 12-15%

[0020] Nano zinc oxide 1-3%

[0021] Modified starch 1-3%

[0022] Carbonate filler 0.5-1.5%

[0023] Defoaming powder 0.8-1.5%

[0024] The balance is synthetic resin glue.

[0025] Water-based resin is a new type of resin system that uses water instead of organic solvent as a dispersion medium. It is fused with water to form a solution, and after the water evaporates, it forms a resin film material. Water-based resin has better film-forming and adhesion properties, and can further improve the adhesion and film-forming properties of low-temperature resistant resins.

[0026] Amino resin is a water-based amino resin with excellent low-temperature resistance, low-temperature adhesion, film-forming property and adhesion. It cooperates with the raw material system of low-temperature resistant resin to further improve the adhesion, low-temperature adhesion and low-temperature resistance of the low-temperature resistant resin.

[0027] Nano zinc oxide can enhance the mechanical properties and anti-aging properties of adhesives. When nano zinc oxide is added to adhesives, it promotes cross-linking between molecules, enhances adhesion and anti-peeling ability. In addition, nano zinc oxide can also increase the UV resistance, antibacterial and water resistance of adhesives, and reduce the possibility of mold and cracking after adhesives are used in cartons.

[0028] The molecular structure of starch is very similar to that of fiber molecules in papermaking fiber raw materials. In addition, it has the advantages of wide sources, low price, and little environmental pollution. Modified starch is a substitute for modified starch. It belongs to ether starch and is a water-soluble anionic polymer compound. It has many advantages such as thickening, bonding, and protective colloid. Therefore, it interacts with water-soluble resins, amino resins, etc. to further improve the adhesion performance of its adhesive, so the corrugated paper produced has better bonding stability.

[0029] Carbonate fillers play a role in filling and reinforcing, enhancing the bonding strength of adhesives. Defoaming powder plays a role in defoaming, reducing the generation of foam. Synthetic resin adhesives have properties such as water resistance, heat resistance, corrosion resistance, and low temperature resistance, and interact with modified starch, water-soluble resin, amino resin, etc. to further increase the film-forming and coagulation properties of low-temperature adhesives in a relatively low temperature environment, making the layer structure of corrugated paper bonded and stable.

[0030] In summary, the present application compounds water-soluble resin, amino resin and synthetic resin glue, and comprehensively combines their properties to further improve their low temperature resistance, bonding, adhesion, etc., and under the action of nano zinc oxide, modified starch, carbonate filler and defoaming powder, the obtained low temperature resistant resin glue has better low temperature resistance, bonding and film forming properties at lower temperatures. When it is used in the adhesive raw material system, it interacts with deformed starch, and the low temperature adhesive prepared is used in the production of corrugated paper, which can be bonded at a lower temperature, stabilize the structure of the corrugated paper, reduce the energy consumption of the production process, and also play a better low temperature resistance, reducing the possibility of cracking of the corrugated paper due to long-term use at low temperatures.

[0031] Preferably, the water-soluble resin is one or more of polyvinyl alcohol resin, water-based polyurethane, and water-soluble alkyd resin.

[0032] Polyvinyl alcohol resin, waterborne polyurethane, and water-soluble alkyd resin are all water-soluble resins, and all have advantages such as film-forming property and adhesion property. Therefore, using one or more of polyvinyl alcohol resin, waterborne polyurethane, and water-soluble alkyd resin can further improve the adhesion property of the low-temperature adhesive.

[0033] Preferably, the amino resin is melamine formaldehyde resin and / or polyamide polyamine epichlorohydrin resin.

[0034] Melamine formaldehyde resin and polyamide polyamine epichlorohydrin resin both have good low temperature resistance, adhesion and film-forming properties at low temperatures, which can reduce energy consumption and stabilize the layer structure of corrugated paper.

[0035] Preferably, the weight ratio of the melamine formaldehyde resin to the polyamide polyamine epichlorohydrin resin is (1-5):1.

[0036] When melamine formaldehyde resin and polyamide polyamine epichlorohydrin resin are compounded, the low-temperature resin adhesive has better low-temperature resistance and adhesion.

[0037] Preferably, the synthetic resin adhesive is an aqueous dispersion of rosin polyol ester resin and / or an aqueous acrylic rosin modified tackifying emulsion.

[0038] The aqueous dispersion of rosin polyol ester resin and the aqueous acrylic rosin modified tackifying emulsion are both modified materials of rosin resin, and have the characteristics of rosin resin, so they have better low temperature resistance and bonding properties, thus further providing the bonding strength and low temperature resistance of the low temperature adhesive, reducing the possibility of cracking of the layer structure of the corrugated paper box after long-term use. And after the aqueous dispersion of rosin polyol ester resin and / or the aqueous acrylic rosin modified tackifying emulsion are mixed with the raw material system of low temperature resin glue, the prepared low temperature resin glue has a lower bonding temperature, so that the low temperature adhesive forms a film at a lower temperature, forming corrugated paper with better bonding strength.

[0039] Preferably, the weight ratio of the rosin polyol ester resin aqueous dispersion to the aqueous acrylic rosin modified tackifying emulsion is (1-5):1.

[0040] When the present application adopts the compounding of the aqueous dispersion of rosin polyol ester resin and the aqueous acrylic rosin modified tackifying emulsion, it can further improve the low-temperature adhesive to obtain better low-temperature resistance, bonding strength and lower film-forming temperature, reduce energy consumption, increase productivity and reduce costs. At the same time, at a lower processing temperature, it can also form a film quickly and improve the bonding stability of the corrugated paper layer structure.

[0041] Preferably, the modified starch is one or more of carboxymethyl starch, hydroxypropyl starch, and acetylated distarch adipic acid.

[0042] Carboxymethyl starch, hydroxypropyl starch, and acetylated distarch adipic acid all play a role in increasing consistency and improving bonding strength. When combined with the raw material system of low-temperature resin glue, they can achieve better bonding strength and low-temperature resistance, and can be bonded at lower temperatures. The resulting corrugated paper layer has a stable structure, reducing the possibility of cracking.

[0043] In a second aspect, the present application provides a method for preparing a low-temperature adhesive, comprising the following steps:

[0044] According to weight parts, 95-102 parts of first water, 13-17 parts of first modified starch, and 4.5-5.5 parts of first washing water are weighed and put into a stirring tank to mix evenly, and then 1-3 parts of second water are added to rinse the inner wall of the stirring tank and stir for 20-35s; then 2-3 parts of low-temperature resin glue are added to mix evenly, and the viscosity is tested. When the viscosity reaches 20-23s, the stirring is stopped; then 21-25 parts of third water and 14-16 parts of second washing water are added, and stirring is continued for 8-15s, and then 13-18 parts of second modified starch are added, and then 1-3 parts of fourth water are added to rinse the inner wall of the stirring tank, and then 0.3-0.5 parts of borax are added, and stirring is continued for 850-1000s, and the corresponding viscosity is tested to obtain a low-temperature adhesive.

[0045] Water, modified starch and washing water are added step by step to ensure that the materials are fully mixed, and water is added again to rinse the inner wall of the mixing kettle to prevent the modified starch from being adsorbed on its inner wall (the inner wall above the water level); after adding the low-temperature resin glue, continue to stir evenly to control its viscosity, and add some water, modified starch, etc. again to ensure that they are fully mixed.

[0046] The solid contents of the first washing water and the second washing water of the present application are both 0.04-0.32%, and the solid contents actually measured in the embodiment are 0.13%.

[0047] The first washing water and the second washing water are both water obtained after the reactor is cleaned after the low-temperature adhesive is produced every day, and the water contains a small amount of low-temperature resin glue, modified starch, and borax. In the embodiments, the first washing water and the second washing water used in each embodiment are the water obtained after the reactor is cleaned in Embodiment 1.

[0048] In a third aspect, a process for producing corrugated paper containing a low-temperature adhesive is prepared by the following method:

[0049] The first base paper is thermoformed to form a corrugated structure, a low-temperature adhesive is sprayed on the surface of the second base paper, and the side containing the adhesive is transferred to the surface of a base paper for bonding, and the thermal bonding is stabilized by a bonding device to form a semi-finished product; a low-temperature adhesive is coated on one side of the adhesive surface of the second base paper raw material of the semi-finished product, and the adhesive surface of the obtained second base paper is transferred to the surface of the third base paper for bonding, and then hot pressing and shearing are performed to obtain corrugated paper.

[0050] The above-mentioned corrugated paper production process obtains a stable corrugated paper structure and high production efficiency. Specifically, the corrugated structure is C-type corrugation, and the first base paper, the second base paper, and the third base paper are all 150-180g / m 2 In the application example, 150g / m 2 The amount of low-temperature adhesive sprayed on both sides of the second base paper is 10-20g / m 2 , the preferred application example is 15g / m 2 The pressing pressure is 2-10N, and 5N is preferred in the application example.

[0051] In summary, this application has the following beneficial effects:

[0052] 1. The present application adopts low-temperature resin glue and modified starch for compounding, and under the action of water and borax, the obtained low-temperature resin adhesive has better adhesion, adhesion, low-temperature resistance, etc. Therefore, when used in the production of corrugated paper, it can be adhered and bonded at a lower temperature, so that the layer structure of the corrugated paper is bonded stably and the possibility of falling off is reduced.

[0053] 2. The present application uses water-soluble resin, amino resin and synthetic resin glue to compound and comprehensively consider their performances, so as to further improve their low temperature resistance, cohesiveness and adhesion, and under the action of nano zinc oxide, modified starch, carbonate filler and defoaming powder, the obtained low temperature resistant resin glue has better low temperature resistance, cohesiveness and film forming property at lower temperature. When it is used in the adhesive raw material system, it interacts with deformed starch, and the low temperature adhesive prepared is used for the production of corrugated paper, which can be bonded at a lower temperature, stabilize the structure of corrugated paper, reduce the energy consumption of the production process, and also play a better low temperature resistance, reducing the possibility of cracking of corrugated paper due to long-term use at low temperature. DETAILED DESCRIPTION

[0054] The present application is further described in detail below in conjunction with embodiments.

[0055] The sources of some raw materials;

[0056] Table 1 Sources of some raw materials

[0057]

[0058]

[0059] Preparation Example of Low Temperature Resin Glue Preparation Example 1

[0060] A low-temperature resin glue is prepared by the following method: 1.5kg of water-soluble resin, 1.2kg of amino resin, 0.1kg of nano zinc oxide, 0.3kg of modified starch, 0.05kg of carbonate filler, 0.08kg of defoaming powder and 6.77kg of synthetic resin glue are weighed and put into a stirring kettle for mixing at a stirring speed of 50r / min and a stirring time of 30min to make them fully mixed and uniform, and the stirring is continued. The mixture is sealed and subjected to reduced pressure distillation at a heating temperature of 75°C and a vacuum gauge showing -0.1Mpa. The solid content is tested during the reduced pressure distillation process. When the solid content reaches 95%, the reduced pressure distillation is stopped and the material is discharged to obtain the low-temperature resin glue.

[0061] The water-soluble resin is polyvinyl alcohol resin.

[0062] Amino resin is melamine formaldehyde resin.

[0063] The synthetic resin glue is an aqueous dispersion of rosin polyol ester resin.

[0064] The carbonate filler is silicon dioxide; the particle size of silicon dioxide and nano zinc oxide is 100 nm.

[0065] Preparation Example 2-12

[0066] Preparation Example 2-12 is different from Preparation Example 1 in that the composition and amount of the raw materials are different, as shown in Table 2;

[0067]

[0068]

[0069]

[0070] Preparation Comparative Example

[0071] Preparation Comparative Example 1

[0072] The difference between the preparation of comparative example 1 and comparative example 1 is that an equal amount of the water-soluble resin is replaced with a synthetic resin glue.

[0073] Preparation Comparative Example 2

[0074] The difference between the preparation of comparative example 2 and comparative example 1 is that the modified starch is replaced with synthetic resin glue in equal amount.

[0075] Preparation Comparative Example 3

[0076] The difference between the preparation of comparative example 3 and comparative example 3 is that the amino resin is replaced with synthetic resin glue in equal amount.

[0077] Preparation Comparative Example 4

[0078] The difference between the preparation of comparative example 4 and comparative example 4 is that the synthetic resin glue is replaced by water-soluble resin in equal amounts.

[0079] Example

[0080] Example 1

[0081] A method for preparing a low-temperature resin adhesive comprises the following steps:

[0082] Weigh 98 kg of the first water, 16 kg of the first modified starch, and 5 kg of the first washing water into a stirring kettle, heat to 30°C, mix at a speed of 120 r / min for 30.0 s, then add 2 kg of the second water to rinse the inner wall of the stirring kettle, rinse the modified starch in the adsorption reactor into the interior of the reactor, and mix with the water inside the reactor, continue stirring for 30 s, and obtain a mixture A.

[0083] Add 2.25kg of low-temperature resin glue to mixture A, continue stirring, and test at the same time. When the test viscosity reaches 22.0S, stop stirring; add 23kg of the third water and 14kg of the second washing water, continue stirring for 10.0s, add 14kg of the second modified starch, add 2kg of the fourth water to rinse the inner wall of the stirring kettle, add 0.4kg of borax, continue stirring for 850s, and when the tested viscosity is 12.0S, stop stirring to obtain a low-temperature adhesive.

[0084] The first water, second water, third water and fourth water mentioned above are all deionized water; the first washing water and the second washing water are both the water used to clean the reactor after the daily production of the low-temperature adhesive is completed, and the water contains a small amount of low-temperature resin glue, modified starch and borax, and its solid content is measured to be 0.13%.

[0085] The first modified starch and the second modified starch are both commercially available modified starches; and the low-temperature resin glue is commercially available.

[0086] Example 2

[0087] The difference between Example 2 and Example 1 is that the preparation of the low-temperature adhesive comprises the following steps:

[0088] Weigh 95 kg of the first water, 13 kg of the first modified starch, and 5 kg of the first washing water, put them into a stirring tank, heat to 30°C, mix at a speed of 120 r / min for 30.0 s, then add 4.5 kg of the second water to rinse the inner wall of the stirring tank, rinse the modified starch in the adsorption reactor into the interior of the reactor, and mix with the water inside the reactor, continue stirring for 30 s, and obtain a mixture A.

[0089] Add 2kg of low-temperature resin glue to mixture A, continue stirring, add 25kg of the third water and 14kg of the second washing water, and test at the same time. When the test viscosity reaches 22.0, stop stirring; continue stirring for 15s, add 18kg of the second modified starch, add 2kg of the fourth water to rinse the inner wall of the stirring kettle, add 0.03kg of borax, continue stirring for 950s, and when the tested viscosity is 12.0S, stop stirring to obtain a low-temperature adhesive.

[0090] Example 3

[0091] Example 3

[0092] The difference between Example 3 and Example 1 is that the preparation of the low-temperature adhesive comprises the following steps:

[0093] Weigh 95 kg of the first water, 13 kg of the first modified starch, and 5 kg of the first washing water, put them into a stirring tank, heat to 30°C, mix at a speed of 120 r / min for 30.0 s, then add 4.5 kg of the second water to rinse the inner wall of the stirring tank, rinse the modified starch in the adsorption reactor into the interior of the reactor, and mix with the water inside the reactor, continue stirring for 30 s, and obtain a mixture A.

[0094] Add 3kg of low-temperature resin glue to mixture A, continue stirring, add 21kg of the third water and 16kg of the second washing water, and test at the same time. When the test viscosity reaches 23.0S, stop stirring; continue stirring for 15s, add 13kg of the second modified starch, add 2kg of the fourth water to rinse the inner wall of the stirring kettle, add 0.05kg of borax, continue stirring for 1000s, and when the tested viscosity is 12.0S, stop stirring to obtain a low-temperature adhesive.

[0095] Example 4-19

[0096] The difference between Example 4-19 and Example 1 is that the source of the low-temperature resin glue is different, as shown in Table 3;

[0097] Table 3 Sources of low temperature resin glue of Examples 4-19

[0098]

[0099]

[0100] Comparative Example

[0101] Comparative Example 1

[0102] The difference between Comparative Example 1 and Example 1 is that the low-temperature resin glue is replaced by phenolic resin in equal amount.

[0103] Comparative Example 2

[0104] The difference between Comparative Example 2 and Example 1 is that the modified starch is replaced by corn starch and the reactor temperature is 60°C.

[0105] Comparative Example 3

[0106] The difference between Comparative Example 3 and Example 1 is that the amount of low-temperature resin glue added is 1 kg.

[0107] Comparative Example 4

[0108] The difference between Comparative Example 4 and Example 1 is that the amount of low-temperature resin glue added is 5 kg.

[0109] Comparative Example 5

[0110] The difference between Comparative Example 5 and Example 1 is that the low-temperature resin glue is EAA copolymer emulsion (German KEIM, Novaseal 2225)

[0111] Performance testing

[0112] The low-temperature adhesives obtained in Examples 1-19 and Comparative Examples 1-5 were subjected to the following performance tests.

[0113] Detection method / test method

[0114] (I) Adhesion strength

[0115] (1) The low-temperature adhesives obtained in Examples 1-19 and Comparative Examples 1-5 were tested for bonding strength according to GB / T 6548-1998, the method for determining bonding strength of corrugated cardboard; the specific data are shown in Table 4.

[0116] (2) The low-temperature adhesives obtained in Examples 1-19 and Comparative Examples 1-5 were subjected to the test samples obtained by placing them in an environment with a humidity of 60% and a temperature of -20°C for 7 days with reference to the method for determining the bonding strength of corrugated board in GB / T 6548-1998. The bonding strength was then tested and the bonding strength change rate was calculated. The bonding strength change rate was equal to the bonding strength obtained in test (1) minus the bonding strength obtained in test (2). The difference was then divided by the bonding strength obtained in test (1), and the remainder was 100%.

[0117] The above experiments were carried out 3 times and the average values ​​were taken. The specific data are shown in Table 4;

[0118] Table 4 Experimental data of Examples 1-19 and Comparative Examples 1-5

[0119]

[0120]

[0121] Combining Example 1 and Comparative Example 1 and Table 4, it can be seen that the bonding strength of Comparative Example 1 is lower than that of Example 1, and the bonding strength change rate of Comparative Example 1 after low-temperature treatment is larger, indicating that the low-temperature resin glue of the present application has better low-temperature resistance and adhesion, and reduces the cracking phenomenon of the corrugated paper layer structure.

[0122] Combining Example 1 and Comparative Example 2 and Table 4, it can be seen that the bonding strength of Comparative Example 2 is lower than that of Example 1, indicating that the modified starch used in the present application is compounded with the low-temperature resin glue of the present application, which can achieve better bonding performance and reduce the possibility of cracking in the corrugated paper layer structure.

[0123] It can be seen from Example 1 and Comparative Examples 3-4 and Table 4 that the bonding strength of Comparative Examples 3-4 is lower than that of Example 1, and the dosage range of the low-temperature resin glue of the present application is better.

[0124] Combining Example 1 and Comparative Example 5 and Table 4, it can be seen that the bonding strength of Comparative Example 5 is lower than that of Example 1, indicating that the low-temperature resin glue of the present application has better bonding strength than the EAA copolymer emulsion.

[0125] Combining Example 1 and Example 4 and Table 4, it can be seen that the bonding strength of Example 1 is lower than that of Example 4, and the bonding strength change rate of Example 1 after low-temperature treatment is larger, indicating that the low-temperature resin glue prepared by the present application has better low-temperature resistance and bonding strength.

[0126] Combining Example 4 and Examples 16-19 and Table 4, it can be seen that the bonding strength of Examples 16-19 is lower than that of Example 4, and the bonding strength change rate of Examples 16-19 after low-temperature treatment is larger, indicating that the low-temperature resin glue prepared by compounding the water-soluble resin, amino resin, modified starch and synthetic resin glue of the present application has better low-temperature resistance and bonding strength.

[0127] Application Examples

[0128] Application Example 1

[0129] A process for producing corrugated paper containing a low-temperature adhesive comprises the following steps:

[0130] The first base paper is thermoformed to form a corrugated structure, and the surface of the second base paper is sprayed with the low-temperature adhesive obtained in Example 1 at a spraying amount of 15 g / m 2and conveying the side containing the adhesive to the surface of a base paper for bonding, and making the thermal bonding stable through the bonding device to form a semi-finished product; coating one side of the adhesive surface of the second base paper raw material of the semi-finished product with the low-temperature adhesive obtained in Example 1, conveying the adhesive surface of the obtained second base paper to the surface of the third base paper for bonding, and then performing hot pressing and shearing to obtain corrugated paper.

[0131] The corrugated structure is C-type corrugated, and the first base paper, the second base paper, and the third base paper are all 150-180g / m 2 In the application example, 150g / m 2 The amount of low-temperature adhesive sprayed on both sides of the second base paper is 10-20g / m 2 , the preferred application example is 15g / m 2 The pressing pressure is 2-10N, preferably 5N in Application Example 1, the pressing time is 1s, the pressing temperature is 102°C, and the room temperature is 5°C.

[0132] Application Example 2-24

[0133] The difference between Application Example 2-24 and Application Example 1 is that the source of the low-temperature adhesive is different, as shown in Table 4;

[0134] Table 4 Sources of low temperature adhesives for application examples 1-24

[0135]

[0136]

[0137] Performance testing

[0138] Detection method / test method

[0139] (III) Lamination stability

[0140] The corrugated paper obtained in Application Example 1-24 was cut into test samples of 20cm*20cm, and then the test samples were loaded with 500g, and then the test samples were freely dropped from a height of 2m, the room temperature was 28℃, the humidity was 62%, the edges of the corrugated paper were facing the bottom surface, and one of the edges was in contact with the bottom surface, and the corrugated paper layer structure was observed to see if it was cracked. If cracking occurred, it was recorded as unqualified, and if there was no cracking, it was recorded as qualified;

[0141] Table 5 Experimental data of application examples 1-24

[0142]

[0143]

[0144] Combining Application Example 1, Application Example 20 and Application Example 24 and Table 4, it can be seen that cracking occurred in Application Example 20 and Application Example 24, indicating that under the production process of corrugated paper in the present application, the resin glue with a higher curing temperature, such as phenolic resin, EAA resin (EAA copolymer emulsion), cannot be cured well, resulting in unstable bonding of the corrugated paper layer structure, which is prone to cracking and affects the quality of the corrugated paper.

[0145] It also shows that the low-temperature resin glue of the present application can be thermally bonded at a relatively low temperature. Therefore, when producing corrugated paper in winter, the temperature can be better controlled at its relatively low processing temperature, while reducing energy consumption, and can further improve the uniformity of heating of the corrugated paper, so that each part is heated evenly. Usually the processing temperature in winter is around 110°C, and the heating temperature in summer is selected to be around 95°C. If the scheme of Application Example 20 is adopted, its winter bonding temperature must be at least 120°C to reach the bonding temperature of its layer structure, while the scheme of Application Example 24 must have a winter bonding temperature of at least 150°C. In contrast, the processing temperature of the low-temperature adhesive of the present application is relatively low, and the processing process is easy to control, and the layer structure of the obtained corrugated paper is relatively stable.

[0146] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A low temperature adhesive, characterized in that: It is composed of the following raw materials in parts by weight: Modified starch 25-38 parts 2-3 parts of low temperature resin glue Borax 0.3-0.5 parts 135-150 parts of water; The low temperature resin glue is composed of the following raw materials in percentage by weight: Water-soluble resin 15-23% Amino resin 12-15% Nano zinc oxide 1-3% Modified starch 1-3% Carbonate filler 0.5-1.5% Defoaming powder 0.8-1.5% The balance is synthetic resin glue; The water-soluble resin is one or more of polyvinyl alcohol resin, water-based polyurethane, and water-soluble alkyd resin; The modified starch is one or more of carboxymethyl starch, hydroxypropyl starch, and acetylated distarch adipic acid; The amino resin is composed of melamine formaldehyde resin and polyamide polyamine epichlorohydrin resin in a weight ratio of (1-5): 1; The synthetic resin adhesive is composed of a rosin polyol ester resin aqueous dispersion and an aqueous acrylic rosin modified tackifying emulsion in a weight ratio of (1-5):

1.

2. A method for preparing a low-temperature adhesive as claimed in claim 1, characterized in that: The following steps are involved: According to weight parts, 95-102 parts of first water, 13-17 parts of first modified starch, and 4.5-5.5 parts of first washing water are weighed and put into a stirring tank to mix evenly, and then 1-3 parts of second water are added to rinse the inner wall of the stirring tank and stir for 20-35s; then 2-3 parts of low-temperature resin glue are added to mix evenly, and the viscosity is tested. When the viscosity reaches 20-23s, the stirring is stopped; then 21-25 parts of third water and 14-16 parts of second washing water are added, and stirring is continued for 8-15s, and then 13-18 parts of second modified starch are added, and then 1-3 parts of fourth water are added to rinse the inner wall of the stirring tank, and then 0.3-0.5 parts of borax are added, and stirring is continued for 850-1000s, and the corresponding viscosity is tested to obtain a low-temperature adhesive.

3. A process for producing corrugated paper containing a low-temperature adhesive according to claim 1, characterized in that: Prepared by the following method: The first base paper is thermoformed to form a corrugated structure, a low-temperature adhesive is sprayed on the surface of the second base paper, and the side containing the adhesive is transferred to the surface of a base paper for bonding, and the thermal bonding is stabilized by a bonding device to form a semi-finished product; a low-temperature adhesive is coated on one side of the adhesive surface of the second base paper raw material of the semi-finished product, and the adhesive surface of the obtained second base paper is transferred to the surface of the third base paper for bonding, and then hot pressing and shearing are performed to obtain corrugated paper.