A reactive hot melt adhesive film with high bonding strength and its preparation method and application

By using a branched structure reactive hot melt adhesive film in automotive ceiling fabric bonding technology, combining EVA resin and modified petroleum resin, the existing hot melt adhesive bonding strength and heat resistance are solved, and the problem of insufficient heat resistance is achieved. Low temperature fit and high bond strength, suitable for high-end fabrics such as suede and improves the heat resistance of the fabric.

CN118222213BActive Publication Date: 2024-11-12FOSHAN DINGSHENG POLYMER TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410440113.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-12
Publication Date
2024-11-12
Estimated Expiration
2044-04-12

AI Technical Summary

Technical Problem

In the existing automotive ceiling fabric bonding technology, the bonding strength and heat resistance of hot melt adhesives are insufficient, especially for high-end fabrics such as suede, which are not resistant to high temperatures, and traditional hot melt adhesives are not friendly to the environment, and solvent-based hot melt adhesives The solvents have safety hazards for the human body. The single-component solvent-free hot melt adhesive has low bond strength and poor heat resistance.

Method used

A reactive hot melt adhesive film containing thermoplastic resin, tackifying resin, isocyanate curing agent, mixed polyester polyol and chain extender is used to form a branched structure by mixing branched polyester polyol and polyester polyol. Combining EVA resin and modified petroleum resin, the viscosity and fluidity are regulated, and the bonding strength and heat resistance are improved.

Benefits of technology

It achieves low-temperature bonding and non-scalding fabrics, has high bonding strength and excellent heat resistance, and is suitable for automotive ceiling fabric bonding, improving the performance stability and application range of reactive hot melt adhesive films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004788861350000091
    Figure BDA0004788861350000091
Patent Text Reader

Abstract

The present invention provides a reactive hot melt adhesive film with high bonding strength and a preparation method and application thereof, wherein the reactive hot melt adhesive film comprises the following raw materials in parts by weight: 5 to 10 parts of thermoplastic resin, 5 to 30 parts of tackifying resin, 10 to 25 parts of isocyanate curing agent, 20 to 100 parts of mixed polyester polyol and 10 to 15 parts of chain extender; wherein the mixed polyester polyol is branched polyester polyol and polyester polyol, and the mass ratio of the two is 1: (1.2 to 1.5). The reactive adhesive film has a low bonding temperature, is easy to apply glue, is particularly suitable for bonding automobile ceiling fabrics, does not burn the fabrics, has high bonding strength and excellent heat resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of reactive hot melt adhesive preparation, and in particular relates to a reactive hot melt adhesive film with high bonding strength, a preparation method and application thereof. Background Art

[0002] In the existing field of automobile ceiling fabric decoration, many textile hot melt adhesives are used, mainly including five categories: thermoplastic polyurethane hot melt adhesive film, ethylene-vinyl acetate copolymer hot melt adhesive film, polyester hot melt adhesive film and polyolefin hot melt adhesive film. In response to the technical requirements for laminating fabrics for automobile ceilings, a one-step method using crude MDI may be included. The advantages of this method are mature technology and low cost. The disadvantages are that the curing temperature required during curing is as high as 190°C and the curing time is 2 to 3 minutes, which conventional fabrics can withstand. However, some high-end fur fabrics, such as suede, are not resistant to high temperatures, which causes great damage to the fabric and greatly reduces the decorative effect. The two-step process involves first making the other parts of the ceiling except the fabric in a one-step manner, and then laminating the fabric. Commonly used laminating hot melt adhesives are mainly polyurethane hot melt adhesives, including solvent polyurethane adhesives, water-based polyurethane adhesives and polyester adhesive films. The above hot melt adhesives have a low lamination curing temperature and do not burn or damage the fabric. However, solvent-based polyurethane adhesives are environmentally unfriendly, and water-based polyurethane adhesives are single-sidedly constructed, resulting in poor bonding strength and heat resistance of the fabric. Polyester adhesive films are non-reactive hot melt adhesives with poor heat resistance.

[0003] The patent with application number 202110116087.9 discloses a one-component solvent-free hot melt adhesive for automobile ceilings and a preparation method thereof. It does not require the addition of organic solvents and bisphenol A substances, which solves the problem that solvent-based hot melt adhesives in the prior art have large environmental pollution and potential safety hazards to the human body. It also solves the problem that the tensile strength and peel strength of solvent-free hot melt adhesives in the prior art are low. However, the one-component hot melt adhesive is limited by the cross-linked structure, and has low bonding strength and poor heat resistance; the patent with application number 202110551844.5 discloses a high-temperature resistant reactive polyurethane hot melt adhesive and a preparation method and application thereof. The components of the high-temperature resistant reactive polyurethane hot melt adhesive include a prepolymer, a tackifying resin, a bisphenol A type chain extender, an antioxidant and other additives; the prepolymer is formed by mixing and reacting polyester polyols, polyether polyols and isocyanates, and is used for the composite of automobile ceiling fabrics. It has excellent high-temperature resistance and peel resistance. However, the prepolymer prepared by blending polyester polyols and polyether polyols has relatively poor adhesion.

[0004] Therefore, it is particularly important for the present invention to develop a reactive hot melt adhesive film with high bonding strength. Summary of the invention

[0005] In view of the defects of the prior art, the purpose of the present invention is to provide a reactive hot melt adhesive film with high bonding strength and a preparation method and application thereof. The reactive adhesive film has a low bonding temperature and is easy to apply glue. It is particularly suitable for bonding car ceiling fabrics without damaging the fabrics. It has high bonding strength and excellent heat resistance.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] On one hand, the present invention provides a reactive hot melt adhesive film with high bonding strength, the reactive hot melt adhesive film comprising the following raw materials in parts by weight: 5 to 10 parts of a thermoplastic resin, 5 to 30 parts of a tackifying resin, 10 to 25 parts of an isocyanate curing agent, 20 to 100 parts of a mixed polyester polyol, and 10 to 15 parts of a chain extender;

[0008] Wherein, the mixed polyester polyol is branched polyester polyol and polyester polyol, and the mass ratio of the two is 1:(1.2-1.5).

[0009] Preferably, the mass ratio of the branched polyester polyol to the polyester polyol is 1:1.3.

[0010] In some embodiments of the present invention, the preparation steps of the branched polyester polyol are as follows:

[0011] (1) Adding glycolic acid and ethylenediamine into a reactor, heating to 100-150° C. under an inert atmosphere, reacting for 1-3 hours, and then heating to 150-180° C. for vacuum dehydration for 0.5-2 hours, and obtaining diol after recrystallization;

[0012] (2) Succinic acid, the diol in step (1) and pentaerythritol are added to a reactor in sequence, the temperature is raised to a molten state under an inert atmosphere, a catalyst is added, the temperature is raised to 180-210° C. with stirring, the reaction is carried out for 1-3 hours, and a branched polyester polyol is obtained by evacuating the reactor.

[0013] Preferably, the preparation steps of the branched polyester polyol are as follows:

[0014] (1) Adding glycolic acid and ethylenediamine into a reactor, heating to 130° C. under nitrogen, reacting for 2 h, and then heating to 160° C. for vacuum dehydration for 12 h, and obtaining diol after recrystallization;

[0015] (2) Succinic acid, the diol in step (1) and pentaerythritol are added to a reactor in sequence, the temperature is raised to a molten state under a nitrogen atmosphere, a catalyst is added, the temperature is raised to 195° C. with stirring, the reaction is carried out for 2 h, and a branched polyester polyol is obtained by evacuating the reactor.

[0016] In some embodiments of the present invention, the molar ratio of hydroxyacetic acid to ethylenediamine in step (1) is (2-2.2):1, and the molar ratio of succinic acid in step (2), the diol in step (1) and pentaerythritol is 1.3:(1.1-1.3):0.06.

[0017] Preferably, the molar ratio of glycolic acid to ethylenediamine in step (1) is 2.1:1, and the molar ratio of succinic acid in step (2), the diol in step (1) and pentaerythritol is 1.3:1.2:0.06.

[0018] Preferably, the catalyst is tetrabutyl titanate, and the amount of the catalyst added is 0.1-1% of the total mass of succinic acid, diol and pentaerythritol.

[0019] Further preferably, the added amount of the catalyst is 0.5% of the total mass of succinic acid, diol and pentaerythritol.

[0020] The present invention preferably prepares polyester polyols containing branched structures by esterification and condensation reaction of dibasic acids, diols and polyols with shorter carbon chains, which effectively ensures the content of functional ester bonds and enables the prepared reactive hot melt adhesive to have a molecular chain structure with better tolerance.

[0021] In some embodiments of the present invention, the polyester polyol is one or more of polyhexanediol adipate diol, polycaprolactone diol, polyneopentyl terephthalate diol and polyhexanediol carbonate diol.

[0022] Preferably, the polyester polyol is polyhexamethylene adipate diol.

[0023] More preferably, the number average molecular weight of the polyester polyol is 2000.

[0024] The applicant utilizes the property of polyester polyols that they have a good wetting effect on the substrate, and by adjusting the mixing ratio of branched polyester polyols and polyester polyols in the mixed polyester polyols, the resulting reactive hot melt adhesive with a branched structure has a low viscosity, good fluidity, and is easy to spread evenly. This is because, compared to the linear polyester polyols in the prior art, the hot melt adhesive body obtained by the cross-linking reaction of the polyester polyols with a branched structure and isocyanate has a three-dimensional structure, with less entanglement and cross-linking between chain segments and weak interaction, so the viscosity is low. At the same time, it plays a certain coordinating role in the curing stability problem caused by the strong polarity and thixotropy of the ester bonds of the polyester polyols.

[0025] In some embodiments of the present invention, the thermoplastic resin is EVA resin.

[0026] The present invention preferably uses EVA resin as the film-forming resin, and uses its excellent heat resistance as a carrier for the curing and cross-linking reaction, thereby meeting the requirements for stirring and extrusion temperature during the preparation of the reactive hot melt adhesive and improving the performance stability of the prepared reactive hot melt adhesive film.

[0027] In some embodiments of the present invention, the tackifying resin is a modified petroleum resin, and the preparation steps are as follows:

[0028] Add C5 petroleum resin and silane modifier into the reactor, introduce protective gas, stir evenly, heat to 150-170°C, slowly add initiator, continue to heat to 200-220°C, keep warm for 1-2h, adjust pH to weak alkaline, stir for 10-20min, cool to room temperature, soak, extract and dry to obtain modified petroleum resin.

[0029] Preferably, the preparation steps of the modified petroleum resin are as follows:

[0030] Add C5 petroleum resin and silane modifier into the reactor, introduce nitrogen, stir evenly, heat to 160°C, slowly add initiator, continue to heat to 210°C, keep warm for 1.5 hours, add sodium hydroxide to adjust the pH to weak alkalinity, stir for 15 minutes, cool to room temperature, soak in deionized water, extract with xylene, and dry at 40-60°C for 3-6 hours to obtain modified petroleum resin.

[0031] Preferably, the mass ratio of the C5 petroleum resin to the silane modifier is 1:(0.04-0.1), and the silane modifier is isocyanate propyl triethoxy silane.

[0032] Further preferably, the mass ratio of the C5 petroleum resin to the silane modifier is 1:0.07.

[0033] Preferably, the initiator is dicumyl peroxide, and the added amount of the initiator is 0.5-1% of the total mass of the C5 petroleum resin and the silane modifier.

[0034] Further preferably, the added amount of the initiator is 0.7% of the total mass of the C5 petroleum resin and the silane modifier.

[0035] In some embodiments of the present invention, the mass ratio of the thermoplastic resin to the tackifying resin is 1:(1-3).

[0036] Preferably, the mass ratio of the thermoplastic resin to the tackifying resin is 1:2.

[0037] C5 petroleum resin is the most commonly used type of tackifying resin in the prior art. The applicant has achieved a balance between viscosity and dispersibility by introducing polar groups into the main chain of the petroleum resin, and the introduction of the silane modifier has also significantly improved the adhesion of the C5 petroleum resin. The applicant has also increased the compatibility of the components by regulating the mass ratio of the thermoplastic resin and the tackifying resin to increase the degree of mutual diffusion between the cross-linked interface chain segments of the reactive substances in the reactive hot melt adhesive.

[0038] Preferably, the isocyanate is one or more of alicyclic diisocyanate and aromatic diisocyanate.

[0039] More preferably, the isocyanate is diphenylmethane-4,4'-diisocyanate.

[0040] The use of blocked isocyanate meets the characteristics of reactive hot melt adhesive film. When heated at low temperature, it can preferentially react with moisture in the air to generate a compound containing active hydrogen, which then continues to react with polyols, thereby increasing the crosslinking degree of the system and thus improving the bonding effect.

[0041] Preferably, the chain extender is at least one of trimethylolpropane, ethylenediamine, dimethylthiotoluenediamine, 1,4-butanediol and glycerol.

[0042] More preferably, the chain extender is glycerol.

[0043] The addition of a small molecular weight chain extender produces a chain extension reaction to increase the molecular weight of the polyester polyol and then the molecular weight of the reactive hot melt adhesive, which can improve its cohesion and significantly increase its bonding strength; the polyester polyol under the preferred molecular weight has good flexibility and better adhesion to different substrates, which increases the application range of the reactive hot melt adhesive film.

[0044] On the other hand, the present invention provides a method for preparing a reactive hot melt adhesive film with high bonding strength, comprising the following steps: adding a thermoplastic resin, a tackifying resin and a mixed polyester polyol into a reactor, stirring evenly at 100-120° C., adding an isocyanate curing agent and mixing at ≤90° C., stirring evenly, and when the -NCO content reaches a theoretical set value of 1.5-3wt%, introducing a protective gas to discharge the material, and packaging to obtain the reactive hot melt adhesive film.

[0045] Preferably, the protective gas described in the present invention is nitrogen.

[0046] In another aspect, the present invention provides an application of a reactive hot melt adhesive film with high bonding strength in laminating hot melt adhesive to automobile ceiling fabrics.

[0047] Compared with the prior art, the present invention has the following beneficial effects:

[0048] (1) The reactive hot melt adhesive film with high bonding strength provided by the present invention is preferably prepared by esterification and condensation reaction of dibasic acids, diols and polyols with shorter carbon chains to obtain polyester polyols with branched structures, which are mixed with polyester polyols for use. The reactive hot melt adhesive with branched structures obtained in the end has low viscosity, good fluidity, easy and uniform adhesive spreading, and a molecular chain structure with excellent tolerance and stable curing.

[0049] (2) The reactive hot melt adhesive film with high bonding strength provided by the present invention preferably uses EVA resin as the film-forming resin and uses its excellent heat resistance as a carrier for the curing and cross-linking reaction, thereby meeting the requirements for stirring and extrusion temperature during the preparation of the reactive hot melt adhesive and improving the performance stability of the prepared reactive hot melt adhesive film; by introducing polar groups into the main chain of the petroleum resin, a balance between viscosity and dispersibility is achieved, while improving the adhesion of the C5 petroleum resin; the applicant also increases the compatibility of the components by regulating the mass ratio of the thermoplastic resin and the tackifying resin to increase the degree of mutual diffusion between the cross-linking interface segments of the reactive substances in the reactive hot melt adhesive.

[0050] (3) The reactive hot melt adhesive film with high bonding strength provided by the present invention also adds small molecular weight propylene glycol to increase the molecular weight of the reactive hot melt adhesive, improve its cohesive force, and significantly increase its bonding strength. The polyester polyol under the preferred molecular weight distribution has good flexibility and better adhesion to different substrates, thereby increasing the application range of the reactive hot melt adhesive film. DETAILED DESCRIPTION

[0051] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0052] If not otherwise specified, the reagents used below can be easily obtained from commercial companies, wherein poly(hexamethylene adipate diol) (number average molecular weight of 2000) was purchased from Shanghai MacLean Biochemical Technology Co., Ltd., and EVA resin was purchased from Suzhou Xinlilong Plastic Chemical Co., Ltd.

[0053] Preparation Example 1

[0054] The preparation steps of branched polyester polyol I are as follows:

[0055] (1) Add 2.1 mol of hydroxyacetic acid and 1 mol of ethylenediamine into a reactor, heat to 130° C. under nitrogen, react for 2 h, continue to heat to 160° C. for vacuum dehydration for 12 h, and obtain diol after recrystallization;

[0056] (2) Add 1.3 mol of succinic acid, 1.2 mol of diol and 0.06 mol of pentaerythritol into a reactor, heat to a molten state under a nitrogen atmosphere, add tetrabutyl titanate, stir and heat to 195° C., react for 2 h, and evacuate to obtain branched polyester polyol I;

[0057] The amount of tetrabutyl titanate added is 0.5% of the total mass of succinic acid, diol and pentaerythritol in step (2).

[0058] Preparation Example 2

[0059] The preparation steps of branched polyester polyol II are the same as those of Preparation Example 1, except that in step (2), 1.3 mol of succinic acid and 1.1 mol of diol are added to the reactor.

[0060] Preparation Example 3

[0061] The preparation steps of branched polyester polyol III are the same as those of Preparation Example 1, except that in step (2), 1.3 mol of succinic acid and 1.4 mol of diol are added to the reactor.

[0062] Preparation Example 4

[0063] The preparation steps of modified petroleum resin I are as follows: add 100g C5 petroleum resin and 7g isocyanate propyl triethoxysilane into a reactor, introduce nitrogen, stir evenly, heat to 160°C, slowly drop 0.75g diisopropyl peroxide, continue to heat to 210°C, keep the reaction for 1.5h, add sodium hydroxide to adjust the pH to weak alkalinity, stir for 15min, cool to room temperature, soak in deionized water, extract with xylene, and dry at 50°C for 4.5h to obtain modified petroleum resin I.

[0064] Preparation Example 5

[0065] The preparation steps of modified petroleum resin II are the same as those of Preparation Example 4, except that 100 g of C5 petroleum resin and 4 g of isocyanate propyltriethoxysilane are added to the reactor.

[0066] Preparation Example 6

[0067] The preparation steps of modified petroleum resin II are the same as those of Preparation Example 4, except that 100 g of C5 petroleum resin and 15 g of isocyanate propyltriethoxysilane are added to the reactor.

[0068] Example 1

[0069] A method for preparing a reactive hot melt adhesive film with high bonding strength comprises the following steps, measured in parts by weight: adding 7.5 parts of EVA resin, 15 parts of modified petroleum resin I, 26 parts of branched polyester polyol I, 34 parts of polyhexanediol adipate diol and 12.5 parts of propylene glycol into a reactor, stirring evenly at 110° C., adding 17.5 parts of isocyanate curing agent and mixing at 90° C., stirring evenly, when the -NCO content reaches a theoretical set value of 2.2wt%, introducing nitrogen to discharge the material, and packaging to obtain the reactive hot melt adhesive film.

[0070] Example 2

[0071] A method for preparing a reactive hot melt adhesive film with high bonding strength comprises the following steps, measured in parts by weight: adding 5 parts of EVA resin, 5 parts of modified petroleum resin I, 9 parts of branched polyester polyol I, 11 parts of polyhexane adipate diol and 10 parts of propylene glycol to a reactor, stirring evenly at 110° C., adding 10 parts of diphenylmethane-4,4'-diisocyanate and mixing at 90° C., stirring evenly, when the -NCO content reaches a theoretical set value of 2.2wt%, introducing nitrogen to discharge the material, and packaging to obtain the reactive hot melt adhesive film.

[0072] Example 3

[0073] A method for preparing a reactive hot melt adhesive film with high bonding strength comprises the following steps, measured in parts by weight: adding 10 parts of EVA resin, 5 parts of modified petroleum resin I, 43 parts of branched polyester polyol I, 57 parts of polyhexane adipate diol and 15 parts of propylene glycol to a reactor, stirring evenly at 110° C., adding 25 parts of diphenylmethane-4,4'-diisocyanate and mixing at 90° C., stirring evenly, when the -NCO content reaches a theoretical set value of 2.2wt%, introducing nitrogen to discharge the material, and packaging to obtain the reactive hot melt adhesive film.

[0074] Example 4

[0075] A method for preparing a reactive hot melt adhesive film with high bonding strength, the specific implementation method is the same as that of Example 1, except that 28.6 parts of branched polyester polyol I and 31.4 parts of polyhexamethylene adipate diol are added.

[0076] Example 5

[0077] A method for preparing a reactive hot melt adhesive film with high bonding strength, the specific implementation method is the same as that of Example 1, except that 23 parts of branched polyester polyol I and 37 parts of poly(hexamethylene adipate) glycol are added.

[0078] Example 6

[0079] A method for preparing a reactive hot melt adhesive film with high bonding strength, the specific implementation method is the same as that of Example 1, except that 6.3 parts of modified petroleum resin I are added.

[0080] Example 7

[0081] A method for preparing a reactive hot melt adhesive film with high bonding strength, the specific implementation method is the same as that of Example 1, except that 30 parts of modified petroleum resin I are added.

[0082] Example 8

[0083] A method for preparing a reactive hot melt adhesive film with high bonding strength, the specific implementation method is the same as that of Example 1, except that branched polyester polyol II is used to replace branched polyester polyol I in equal amounts.

[0084] Example 9

[0085] A method for preparing a reactive hot melt adhesive film with high bonding strength, the specific implementation method is the same as that of Example 1, except that branched polyester polyol III is used to replace branched polyester polyol I in equal amounts.

[0086] Example 10

[0087] A method for preparing a reactive hot melt adhesive film with high bonding strength, the specific implementation method is the same as that of Example 1, except that the modified petroleum resin I is replaced by an equal amount of modified petroleum resin II.

[0088] Embodiment 11

[0089] A method for preparing a reactive hot melt adhesive film with high bonding strength, the specific implementation method is the same as that of Example 1, except that the modified petroleum resin III is used to replace the modified petroleum resin I in equal amounts.

[0090] Comparative Example 1

[0091] A method for preparing a reactive hot melt adhesive film with high bonding strength comprises the following steps, measured in parts by weight: adding 7.5 parts of EVA resin, 15 parts of modified petroleum resin I, 60 parts of branched polyester polyol I and 12.5 parts of propylene glycol into a reactor, stirring evenly at 110° C., adding 17.5 parts of isocyanate curing agent and mixing at 90° C., stirring evenly, when the -NCO content reaches a theoretical set value of 2.2wt%, introducing nitrogen to discharge the material, and packaging to obtain the reactive hot melt adhesive film.

[0092] Comparative Example 2

[0093] A method for preparing a reactive hot melt adhesive film with high bonding strength comprises the following steps, measured in parts by weight: adding 7.5 parts of EVA resin, 15 parts of modified petroleum resin I, 60 parts of polyhexane adipate diol and 12.5 parts of propylene glycol to a reactor, stirring evenly at 110° C., adding 17.5 parts of isocyanate curing agent and mixing at 90° C., stirring evenly, when the -NCO content reaches a theoretical set value of 2.2wt%, introducing nitrogen to discharge the material, and packaging to obtain the reactive hot melt adhesive film.

[0094] Example 12

[0095] A method for preparing a reactive hot melt adhesive film with high bonding strength, the specific implementation method is the same as that of Example 1, except that an equal amount of C5 petroleum resin is used to replace the modified petroleum resin I.

[0096] Performance Test:

[0097] Take the reactive adhesive film prepared in the above examples and comparative examples, treat the surface of the automobile ceiling fabric with alcohol, take the reactive hot melt adhesive, apply a coating thickness of 0.4 mm, and compound it with the automobile ceiling fabric. Use a hot press to preheat and press for 30 seconds and hot press for 2 minutes at 50°C, and take out the composite material after cooling. Cut the composite material into several samples of 200mm*25mm, and perform the following performance tests. The specific test results are shown in Table 1.

[0098] (1) Initial viscosity test: The viscosity of the examples was tested using a Brookfield viscometer, model DV2T, with the viscosity controlled at 120°C.

[0099] (2) Final adhesive strength test: After curing for 7 days, the shear strength is the final adhesive strength;

[0100] (3) Slip performance test: Apply glue at 120°C, press for 30 seconds, and test the slip amount under a load of 150g;

[0101] (4) Peel strength test: According to the national standard GB / T 2791-1995, the sample was subjected to a peel strength test, wherein the tensile rate was set to 100 mm / min;

[0102] (5) Heat resistance test: After curing for 7 days, the film was placed in a constant temperature and humidity test chamber at 85°C and 85% RH for aging for 7 days and then peeled off immediately.

[0103] Table 1

[0104]

[0105] As shown in Table 1, the reactive adhesive films prepared in Examples 1 to 3 provided by the present invention have low lamination temperature, suitable viscosity, good fluidity, are easy to apply glue, have high bonding strength and excellent heat resistance, and are particularly suitable for lamination of automobile ceiling fabrics without scalding the fabrics.

[0106] The mass ratio of branched polyester polyol to polyester polyol was changed in Examples 4 and 5. The adhesive force of Example 4 was significantly reduced and it was very easy to peel off, while the initial viscosity of Example 5 was relatively large, and the thixotropy was large, the slip performance was poor, and the stability was not good.

[0107] Examples 6 and 7 change the mass ratio of thermoplastic resin to tackifying resin, which has an adverse effect on the mutual diffusion degree between the cross-linked interface segments of the reactive substances in the reactive hot melt adhesive, resulting in a decrease in the compatibility of the components, thereby affecting the comprehensive performance of the reactive hot melt adhesive film.

[0108] Example 8 and Example 9 changed the monomer ratio of the branched polyester polyol, which had an adverse effect on the content of the functional ester bond and affected the functionality of the branched polyester polyol. The initial viscosity was relatively high, which was not conducive to the subsequent curing and may cause bubble structure, thereby affecting the final adhesion strength.

[0109] Examples 10 and 11 changed the mass ratio of C5 petroleum resin and silane modifier, while Example 12 was unmodified C5 petroleum resin, and their heat resistance decreased significantly. This may be because the dispersibility of the tackifying resin in the system was affected, which was prone to stratification or precipitation and could not provide a stable reaction environment, ultimately affecting the heat resistance and initial adhesion of the reactive hot melt adhesive film.

[0110] Comparative Examples 1 and 2 are comparative examples in which branched polyester polyol I and poly(hexamethylene adipate glycol) ester diol are added separately, respectively, which have adverse effects on the viscosity and fluidity of the system, and both affect the comprehensive performance of the reactive film to a certain extent.

[0111] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A reactive hot melt adhesive film with high bonding strength, characterized in that: The reactive hot melt adhesive film comprises the following raw materials in parts by weight: 5-10 parts of thermoplastic resin, 5-30 parts of tackifying resin, 10-25 parts of isocyanate curing agent, 20-100 parts of mixed polyester polyol and 10-15 parts of chain extender; Wherein, the mixed polyester polyol is branched polyester polyol and polyester polyol, and the mass ratio of the two is 1: (1.2-1.5); The preparation steps of the branched polyester polyol are as follows: (1) Adding glycolic acid and ethylenediamine into a reactor, heating to 100-150° C. under an inert atmosphere, reacting for 1-3 hours, and then heating to 150-180° C. for vacuum dehydration for 0.5-2 hours, and obtaining diol after recrystallization; (2) adding succinic acid, the diol in step (1) and pentaerythritol in sequence to a reactor, heating to a molten state under an inert atmosphere, adding a catalyst, stirring and heating to 180-210° C., reacting for 1-3 hours, and evacuating to obtain a branched polyester polyol; The molar ratio of glycolic acid to ethylenediamine in step (1) is (2-2.2):1, and the molar ratio of succinic acid in step (2), the diol in step (1) and pentaerythritol is 1.3:(1.1-1.3):0.06; The polyester polyol is one or more of polyhexanediol adipate diol, polycaprolactone diol, polyneopentyl terephthalate diol and polyhexanediol carbonate 1,6; The thermoplastic resin is EVA resin; The tackifying resin is a modified petroleum resin, and the preparation steps are as follows: Add C5 petroleum resin and silane modifier into the reactor, introduce protective gas, stir evenly, heat to 150-170°C, slowly drop initiator, continue to heat to 200-220°C, keep warm for 1-2h, adjust pH to weak alkalinity, stir for 10-20min, cool to room temperature, soak, extract and dry to obtain modified petroleum resin; The mass ratio of the C5 petroleum resin to the silane modifier is 1:0.07, and the silane modifier is isocyanate propyl triethoxy silane; The mass ratio of the thermoplastic resin to the tackifying resin is 1:

2.

2. A method for preparing the reactive hot melt adhesive film with high bonding strength as claimed in claim 1, characterized in that: The method comprises the following steps: adding a thermoplastic resin, a tackifying resin and a polyester polyol into a reactor, stirring evenly at 100-120° C., adding an isocyanate curing agent and mixing at ≤90° C., stirring evenly, and when the -NCO content reaches a theoretical set value of 1.5-3wt%, introducing a protective gas to discharge the material, and performing packaging to obtain the reactive hot melt adhesive film.

3. Use of the reactive hot melt adhesive film with high bonding strength as claimed in any one of claims 1 to 2 in hot melt adhesive bonding of automobile ceiling fabrics.

Citation Information

Patent Citations

  • Single-component solventless hot melt adhesive for automobile roof as well as preparation method and use method of single-component solventless hot melt adhesive

    CN112831307A

  • High-temperature-reaction-resistant polyurethane hot melt adhesive and preparation method and application thereof

    CN113201305A

  • Modified polyethylene glycol succinate and preparation methods thereof

    CN103788379A

  • Preparation method of branched waterborne polyurethane nano composite material

    CN108752552A

  • Branched polyester polyol as well as preparation method and application thereof

    CN113150259A