A high-efficiency anti-oxidation silicon crystal nano-surface treatment agent, preparation method and application thereof

By using specially prepared modified particles to coat the silicate surface on the photovoltaic glass panel, combined with graphene, carbon nanotubes and rare earth oxides, a multi-phase coating structure is formed, which solves the problem of shedding and transmittance reduction under wet and freezing conditions. solve the problem, achieve high salt spray resistance and oxidation resistance, extend the service life and improve photovoltaic power generation efficiency.

CN118240405BInactive Publication Date: 2024-10-11DATANG RENEWABLE ENERGY RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410458090.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-16
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing photovoltaic glass panel surface treatment agents are easy to fall off and reduce sunlight transmittance under wet and freezing conditions, and it is difficult to achieve high salt spray resistance and oxidation resistance at the same time, affecting photovoltaic power generation efficiency and service life.

Method used

A specific preparation method is used to coat the modified particles on the silicate surface to form a multi-phase coating structure. It combines graphene, carbon nanotubes and rare earth oxides to optimize the structure and particle size of the composite modified silicate and improve surface modification. The hydrophilicity and light transmittance of the anti-static agent are improved, and metal oxide nanoparticles are introduced to enhance the anti-static property.

Benefits of technology

It significantly improves the frost resistance, salt spray resistance and oxidation resistance of photovoltaic glass, extends its service life, enhances solar light transmittance and self-cleaning performance, and improves photovoltaic power generation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004794834050000151
    Figure BDA0004794834050000151
  • Figure BDA0004794834050000152
    Figure BDA0004794834050000152
  • Figure BDA0004794834050000161
    Figure BDA0004794834050000161
Patent Text Reader

Abstract

The present invention relates to the field of photovoltaic technology, and more specifically, to a high-efficiency anti-oxidation silicon crystal nano-surface treatment agent, a preparation method and an application thereof. The high-efficiency anti-oxidation silicon crystal nano-surface treatment agent comprises 40-60 parts of composite modified silicate, 10-20 parts of polymer solution, 10-20 parts of metal oxide nanoparticle dispersion, 1-5 parts of defoaming agent, and 30-60 parts of water by mass. The obtained high-efficiency anti-oxidation silicon crystal nano-surface treatment agent can improve the service life of photovoltaic glass panels and solve the problem that the external environment affects the overall power generation efficiency of photovoltaic power generation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of photovoltaic technology, and more specifically to a high-efficiency anti-oxidation silicon crystal nano-surface treatment agent, a preparation method and application thereof. Background Art

[0002] In recent years, photovoltaic power generation has become a hot spot for the development of new energy, and photovoltaic panels are the core part of solar photovoltaic power generation systems. In order to increase the service life of photovoltaic glass panels, surface treatment agents are often used to protect photovoltaic glass panels. In addition, the main factor affecting the overall power generation efficiency of photovoltaic power generation is the external environment, including dust, snow, bird droppings and other coverings that affect the sun's radiation to photovoltaic panels and reduce the efficiency of photovoltaic power generation. Therefore, it is of great significance to prepare an effective antioxidant silicon crystal nano-surface treatment agent that can increase the service life of photovoltaic glass panels while improving the power generation efficiency of photovoltaic power generation.

[0003] The Chinese patent with publication number CN117210036A discloses a method for preparing a weather-resistant photovoltaic glass panel coating solution. The mass percentage of each component based on the total mass of the raw materials is as follows: 10%-40% dissolved silica sol, 6%-20% acrylic resin, 0.5%-1% silane coupling agent, 0.5%-2% ethyl orthosilicate, 0.5%-2% methyltriethoxysilane, 1%-3% anhydrous ethanol, 0.5%-2% isopropanol, 0.2%-0.8% additives and 30%-50% deionized water. The weather-resistant photovoltaic glass panel coating liquid provided by the technical solution can prevent the paint surface from oxidation and aging. The real glass coating does not contain petroleum components, and after construction, a hard inorganic film layer will be formed on the surface of the photovoltaic glass, which is tightly combined with the photovoltaic glass and will never fall off. It completely isolates the photovoltaic glass from the air and can effectively prevent the photovoltaic glass from oxidation and discoloration caused by external factors. It is resistant to salt spray. The hard non-organic film layer will not oxidize itself, and it also prevents the external acid rain, flying insects, bird droppings, etc. from causing salt spray on the photovoltaic glass. The dense glass crystal film has super strong resistance to salt spray. However, the film-forming substance acrylic resin in the technical solution will lead to poor flexibility and temperature resistance of the film layer.

[0004] The Chinese patent with the publication number CN115873430A discloses a photovoltaic self-cleaning dustproof and anti-reflective nano coating and its use method, wherein the nano material comprises the following components: 5% by weight of amorphous silicon dioxide, 70% by weight of deionized water, 18% by weight of polyethanol and 6% by weight of surfactant. First, the plasma water is heated, and the amorphous silicon dioxide is placed in the deionized water for stirring and mixing to obtain a mixed solution; then the polyethanol and the surfactant are mixed in the solution and then stirred and mixed, and the mixture is cooled after being completely mixed. The photovoltaic self-cleaning dustproof and anti-reflective nano coating and its use method, the product is applied on the surface of the glass by wiping or spraying, and the product is suitable for the surface of photovoltaic glass, photovoltaic panel, etc., and through the effect of the nano coating, the surface has the functions of self-cleaning, dustproof and anti-reflective, and effectively protects the glass surface and improves the power generation efficiency. However, the nano coating obtained by the technical solution will affect its effect when it comes into contact with water or water vapor in the air. Summary of the invention

[0005] The purpose of the present invention is to provide a high-efficiency anti-oxidation silicon crystal nano-surface treatment agent, a preparation method and its application, so as to improve the service life of photovoltaic glass panels and solve the problem that the external environment affects the overall power generation efficiency of photovoltaic power generation.

[0006] The first aspect of the present invention provides a high-efficiency anti-oxidation silicon crystal nano-surface treatment agent, which comprises, by weight, 40-60 parts of composite modified silicate, 10-20 parts of polymer solution, 10-20 parts of metal oxide nanoparticle dispersion, 1-5 parts of defoaming agent, and 30-60 parts of water;

[0007] The composite modified silicate is a silicate coated with modified particles; the silicate includes alkali metal silicate and layered structure silicate;

[0008] The preparation method of the modified particles comprises the following steps: mixing and stirring the particles in ethanol for 30-60 minutes, then adding N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and aluminum acetate, and reacting at 60-70° C. for 30-60 minutes to obtain the modified particles;

[0009] The particles include graphene, carbon nanotubes, and rare earth oxides in a mass ratio of (10-20):(2-5):(0.05-2);

[0010] The graphene has a wrinkled structure and a thickness of 1-5 nm;

[0011] The carbon nanotubes are a mixture of multi-walled carbon nanotubes with a diameter of 8-20 nm and multi-walled carbon nanotubes with a diameter of 30-60 nm, with a mass ratio of (5-10): (2-5);

[0012] The rare earth oxides are spherical lanthanum oxide with a particle size of 30-50 nm and irregular yttrium oxide with a particle size of 0.5-2 μm, with a mass ratio of (2-3):1;

[0013] The mass ratio of the particles, ethanol, N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and aluminum acetate is (15-25): 150: (0.2-0.6): (0.1-0.5).

[0014] The preparation method of the composite modified silicate comprises the following steps: dispersing the silicate in a 60-80 vol% ethanol aqueous solution by ultrasonication, adding the modified particles under stirring, reacting at 50-70° C. for 6-8 hours, and then drying to obtain the composite modified silicate;

[0015] The mass ratio of the silicate, ethanol aqueous solution and modified particles is (5-10):100:(2-5).

[0016] Preferably, the thickness of the graphene is 2±1 nm.

[0017] Preferably, the carbon nanotubes are a mixture of multi-walled carbon nanotubes with a diameter of 11.5±3.5 nm and multi-walled carbon nanotubes with a diameter of 40±10 nm, with a mass ratio of 8:5.

[0018] Preferably, the rare earth oxides are spherical lanthanum oxide with a particle size of 40 nm and irregular yttrium oxide with a particle size of 1 μm, with a mass ratio of 2:1.

[0019] Preferably, the mass ratio of the silicate, the ethanol aqueous solution and the modified particles is 8:100:4.

[0020] The present invention introduces graphene, carbon nanotubes, and rare earth oxides into the surface modifier, which can improve the power generation efficiency and service life of photovoltaic glass. However, the inventors found in the experimental process that when graphene, carbon nanotubes, and rare earth oxides are simply mixed with silicates, the surface modifier obtained will cause the photovoltaic glass surface coating to fall off easily under wet and frozen conditions, and the effective transmittance of sunlight will decrease. To solve the above problems, the inventors found that the surface modifier can effectively solve the problem that the surface modifier will cause the photovoltaic glass surface coating to crack easily under wet and frozen conditions, and the effective transmittance of sunlight will decrease. The inventors speculate that it is because the modified particles obtained by the specific method are multi-phase coating structures. When they are coated on the silicate surface, the modified particles and the silicate are more closely combined with each other, which increases the affinity between the systems, is conducive to the uniform dispersion of the modified particles in the system, and effectively prevents the agglomeration of the modified particles; at the same time, the obtained composite modified silicate has better structural stability, which can avoid the destruction of the composite modified silicate structure, thereby avoiding the fall of the photovoltaic glass surface coating and improving the wet and frozen resistance.

[0021] The inventors further discovered that when the mass ratio of graphene, carbon nanotubes, and rare earth oxides is (10-20):(2-5):(0.05-2), the graphene has a wrinkled structure and a thickness of 1-5 nm, the carbon nanotubes are a composite of multi-walled carbon nanotubes with a diameter of 8-20 nm and multi-walled carbon nanotubes with a diameter of 30-60 nm, and the rare earth oxides are spherical lanthanum oxide with a particle size of 30-50 nm and irregular yttrium oxide with a particle size of 0.5-2 μm, the obtained surface modifier can improve the salt spray resistance and oxidation resistance of photovoltaic glass when used for photovoltaic glass, and at the same time the surface modifier has good hydrophilicity. The inventors speculate that it is because the modified particles obtained from graphene, carbon nanotubes, and rare earth oxides with specific structures and particle sizes can form a coated multiphase composite porous structure. When the alkali metal silicates and layered silicates coated therewith form a dense protective film on the surface of the photovoltaic glass, the micropores and cracks in the coating are reduced, the permeability of the coating is reduced, and oxygen or salt spray media are effectively prevented from penetrating into the interior of the coating; at the same time, the alkali metal silicates and layered silicates coated by the modified particles reduce the surface energy of the surface modifier while increasing the micro-roughness of the surface of the surface modifier, effectively improving the hydrophilicity of the coating, but failing to achieve super hydrophilicity, and the self-cleaning performance needs to be improved.

[0022] Preferably, the mass ratio of the alkali metal silicate to the layered silicate is (1-3):1.

[0023] Preferably, the alkali metal silicate is selected from at least one of potassium silicate, sodium silicate and lithium silicate, preferably potassium silicate and sodium silicate.

[0024] Preferably, the mass ratio of potassium silicate to sodium silicate is (5-15):(2-8), preferably 12:5.

[0025] Preferably, the layered silicate is selected from at least one of talc, montmorillonite, mica powder and kaolinite, preferably talc and mica powder, with a mass ratio of (1-2): (1-2).

[0026] Preferably, the talcum powder D50 is 5-10 μm, preferably 6.1±0.1 μm.

[0027] Preferably, the mica powder has an aspect ratio of ≥50 and D50 ≤20 μm.

[0028] Preferably, the mica powder has an aspect ratio of 80 and a D50 of 12±2 μm.

[0029] The inventors further discovered that when the alkali metal silicates are potassium silicate and sodium silicate, and the mass ratio of potassium silicate to sodium silicate is controlled to be (5-15):(2-8), and the layered silicate is talcum powder with a D50 of 5-10 μm and mica powder with a diameter-to-thickness ratio of ≥50 and D50≤20 μm, the moisture and heat resistance of the surface modifier can be improved, thereby avoiding affecting the service life of the photovoltaic glass.

[0030] Preferably, the mass ratio of the composite modified silicate to the polymer solution is (45-55):(10-15), preferably 50:12.

[0031] Preferably, the polymer solution is selected from at least one of a polyvinyl alcohol aqueous solution, a polyethylene glycol aqueous solution, and a polyvinyl pyrrolidone aqueous solution.

[0032] Preferably, the polymer solution is a polyvinyl alcohol aqueous solution.

[0033] Preferably, the polyvinyl alcohol is selected from at least one of polyvinyl alcohol PVA100-78, polyvinyl alcohol PVA100-60, and polyvinyl alcohol PVA100-27.

[0034] Preferably, the polyvinyl alcohol is polyvinyl alcohol PVA100-60.

[0035] Preferably, the polyvinyl alcohol PVA100-60 has an alcoholysis degree of 91-100 mol % and a viscosity of 10-30 mPa.s.

[0036] Preferably, the polyvinyl alcohol PVA100-60 has a degree of alcoholysis of 95±1 mol% and a viscosity of 25±3 mPa.s.

[0037] Preferably, the polyvinyl alcohol aqueous solution consists of polyvinyl alcohol and water in a mass ratio of (10-15) : 1000, preferably 12:1000.

[0038] The inventors found that when a polyvinyl alcohol PVA100-60 aqueous solution with a degree of alcoholysis of 91-100 mol% and a viscosity of 10-30 mPa.s is introduced, and the mass ratio of the composite modified silicate to the polymer solution is controlled to be (45-55): (10-15), the obtained surface modifier can solve the super-hydrophilicity of the surface modifier that cannot be achieved by using the composite modified silicate alone, and can improve the cracking performance of the surface modifier at low temperatures while achieving self-cleaning properties. The inventors speculate that it may be because the polyvinyl alcohol and the composite modified silicate undergo a cross-linking reaction to form a more stable network structure, thereby achieving super-hydrophilicity, achieving self-cleaning properties, and this cross-linked network structure can effectively prevent cracks and peeling of the surface modifier at low temperatures.

[0039] Preferably, the metal oxide nanoparticles in the metal oxide nanoparticle dispersion are selected from at least one of titanium dioxide, silicon dioxide, zinc oxide and aluminum oxide.

[0040] Preferably, the metal oxide nanoparticles are a combination of titanium dioxide and zinc oxide.

[0041] Preferably, the mass ratio of titanium dioxide to zinc oxide is (15-20):(10-15), preferably 18:12.

[0042] Preferably, the titanium dioxide is selected from at least one of anatase titanium dioxide, rutile titanium dioxide and mixed crystal titanium dioxide, preferably mixed crystal titanium dioxide.

[0043] Preferably, the particle size of the mixed crystal titanium dioxide is 10-30 nm, preferably 20 nm.

[0044] Preferably, the particle size of the zinc oxide is 30-80 nm, preferably 50 nm.

[0045] Preferably, the method for preparing the metal oxide nanoparticle dispersion comprises the following steps: mixing the metal oxide nanoparticles, a polymer dispersant and water in a mass ratio of (20-30):(1-3):100 and performing ultrasonic dispersion to obtain a uniform dispersion.

[0046] Preferably, the polymer dispersant is a high molecular weight copolymer containing pigment affinity groups.

[0047] The composite modified silicate and polymer solution in the present invention can achieve super hydrophilicity of the surface modifier, but polyvinyl alcohol is sensitive to ultraviolet rays, which will affect the transmittance of the surface modifier when applied to the surface of photovoltaic glass to a certain extent, affecting the photoelectric conversion efficiency. In order to solve the above problems, the present invention introduces a metal oxide nanoparticle dispersion. The inventor unexpectedly found that when the metal oxide nanoparticles are a combination of titanium dioxide and zinc oxide, the titanium dioxide is a mixed crystal titanium dioxide with a particle size of 10-30nm, the particle size of zinc oxide is 30-80nm, and the mass ratio of titanium dioxide to zinc oxide is controlled to be (15-20): (10-15), the obtained surface modifier can improve the transmittance of photovoltaic glass when used for photovoltaic glass. The inventor speculates that this is because the titanium dioxide and zinc oxide under this condition can improve the absorption of ultraviolet rays by the surface modifier while acting together with graphene to form a fine convex-concave structure on the surface of the surface modifier, further increasing the surface roughness of the surface modifier, reducing reflectivity, and improving transmittance.

[0048] Preferably, the defoamer is selected from at least one of an organosilicon defoamer and a fluorocarbon defoamer, preferably an organosilicon defoamer.

[0049] The second aspect of the present invention provides a method for preparing a highly efficient anti-oxidation silicon crystal nano-surface treatment agent, comprising the following steps: mixing and stirring composite modified silicate, polymer solution, metal oxide nano-particle dispersion, defoamer and water to obtain the obtained product.

[0050] The third aspect of the present invention provides an application of a highly efficient anti-oxidation silicon crystal nano-surface treatment agent for the protection of photovoltaic glass.

[0051] Beneficial effects:

[0052] 1. The present invention coats the surface of silicate with modified particles prepared by a specific method, which effectively solves the problem that the surface modifier will cause the surface coating of photovoltaic glass to crack easily under wet and frozen conditions and reduce the effective transmittance of sunlight.

[0053] 2. In the present invention, when the mass ratio of graphene, carbon nanotubes and rare earth oxides is (10-20):(2-5):(0.05-2), the graphene has a wrinkled structure and a thickness of 1-5 nm, the carbon nanotubes are a composite of multi-walled carbon nanotubes with a diameter of 8-20 nm and multi-walled carbon nanotubes with a diameter of 30-60 nm, and the rare earth oxides are spherical lanthanum oxide with a particle size of 30-50 nm and irregular yttrium oxide with a particle size of 0.5-2 μm, the obtained surface modifier can improve the salt spray resistance and oxidation resistance of photovoltaic glass when used for photovoltaic glass, and at the same time the surface modifier has good hydrophilicity.

[0054] 3. In the present invention, when the alkali metal silicates are potassium silicate and sodium silicate, and the mass ratio of potassium silicate to sodium silicate is controlled to be (5-15):(2-8), and the layered silicate is talcum powder with a D50 of 5-10 μm and mica powder with a diameter-to-thickness ratio of ≥50 and D50≤20 μm, the moisture and heat resistance of the surface modifier can be improved, thereby preventing the service life of the photovoltaic glass from being affected.

[0055] 4. When the polyvinyl alcohol PVA100-60 aqueous solution with a degree of alcoholysis of 91-100 mol% and a viscosity of 10-30 mPa.s is introduced into the present invention, and the mass ratio of the composite modified silicate to the polymer solution is controlled to be (45-55): (10-15), the obtained surface modifier can solve the super hydrophilicity of the surface modifier that cannot be achieved by using the composite modified silicate alone, and can improve the cracking performance of the surface modifier at low temperature while achieving self-cleaning properties.

[0056] 5. In the present invention, when the metal oxide nanoparticles are a combination of titanium dioxide and zinc oxide, the titanium dioxide is a mixed crystal titanium dioxide with a particle size of 10-30nm, the particle size of zinc oxide is 30-80nm, and the mass ratio of titanium dioxide to zinc oxide is controlled to be (15-20): (10-15), the obtained surface modifier can improve the light transmittance of photovoltaic glass when used for photovoltaic glass.

[0057] 6. The surface modifier prepared by the present invention also has excellent antistatic properties. DETAILED DESCRIPTION

[0058] In order to better explain the present invention, the following will combine the examples in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. The embodiments described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by those skilled in the art without creative work are within the scope of protection of the present invention.

[0059] Example 1

[0060] Example 1 provides a high-efficiency anti-oxidation silicon crystal nano-surface treatment agent, which comprises, by weight, 50 parts of composite modified silicate, 12 parts of polymer solution, 15 parts of metal oxide nanoparticle dispersion, 2 parts of defoaming agent, and 50 parts of water;

[0061] The composite modified silicate is a silicate coated with modified particles; the silicate includes alkali metal silicate and layered structure silicate;

[0062] The preparation method of the modified particles comprises the following steps: mixing the particles in ethanol for 40 minutes, then adding N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and aluminum acetate, and reacting at 65° C. for 45 minutes to obtain the modified particles;

[0063] The particles include graphene, carbon nanotubes, and rare earth oxides in a mass ratio of 15:4:1;

[0064] The graphene has a wrinkled structure and a thickness of 2±1 nm; it was purchased from Nanjing Jicang Nanotechnology Co., Ltd., model: JCVDG-2-30.

[0065] The carbon nanotubes are a mixture of multi-walled carbon nanotubes with a diameter of 11.5±3.5 nm and multi-walled carbon nanotubes with a diameter of 40±10 nm, with a mass ratio of 8:5; they are purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., and the models are: XFM10 and XFM28 respectively.

[0066] The rare earth oxides are spherical lanthanum oxide with a particle size of 40 nm and irregular yttrium oxide with a particle size of 1 μm, with a mass ratio of 2:1; they are purchased from Yijin New Materials.

[0067] The mass ratio of the particles, ethanol, N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and aluminum acetate is 20:150:0.4:0.3.

[0068] The preparation method of the composite modified silicate comprises the following steps: dispersing the silicate in a 70 vol% ethanol aqueous solution by ultrasonication, adding the modified particles under stirring, reacting at 60° C. for 7 hours, and then drying to obtain the composite modified silicate;

[0069] The mass ratio of the silicate, the ethanol aqueous solution and the modified particles is 8:100:4.

[0070] The mass ratio of the alkali metal silicate to the layered silicate is 2:1.

[0071] The alkali metal silicates are potassium silicate and sodium silicate.

[0072] The mass ratio of the potassium silicate to the sodium silicate is 12:5.

[0073] The layered silicate is talcum powder and mica powder, with a mass ratio of 1:1.

[0074] The mica powder has an aspect ratio of 80 and a D50 of 12±2 μm and is purchased from Guangdong Yongfeng Chemical Co., Ltd. Model: ZR-C2.

[0075] The talcum powder D50 is 6.1±0.1 μm and is customized from Quanzhou Yiluoke New Materials Co., Ltd.

[0076] The polymer solution is a polyvinyl alcohol aqueous solution.

[0077] The polyvinyl alcohol is polyvinyl alcohol PVA100-60.

[0078] The polyvinyl alcohol PVA100-60 has a degree of alcoholysis of 95±1 mol% and a viscosity of 25±3 mPa.s and was purchased from Guangzhou Jingyi New Materials Co., Ltd., model: 094-27.

[0079] The polyvinyl alcohol aqueous solution consists of polyvinyl alcohol and water in a mass ratio of 12:1000.

[0080] The metal oxide nanoparticles in the metal oxide nanoparticle dispersion are a combination of titanium dioxide and zinc oxide.

[0081] The mass ratio of titanium dioxide to zinc oxide is 18:12.

[0082] The titanium dioxide is mixed crystal titanium dioxide.

[0083] The mixed crystal titanium dioxide has a particle size of 20 nm and is purchased from Brofos Nanotechnology (Ningbo) Co., Ltd., model: Brofos-TiO2-RJ20.

[0084] The zinc oxide has a particle size of 50 nm and is purchased from Brofos Nanotechnology (Ningbo) Co., Ltd., model: Brofos-ZnO-50.

[0085] The preparation method of the metal oxide nanoparticle dispersion comprises the following steps: mixing the metal oxide nanoparticles, a polymer dispersant and water at a mass ratio of 25:2:100 and performing ultrasonic dispersion to uniformly obtain the dispersion.

[0086] The polymer dispersant is a high molecular weight copolymer containing pigment affinity groups, model: BYK-9077.

[0087] The defoamer is an organosilicon defoamer, model: BYK-024.

[0088] A method for preparing a high-efficiency anti-oxidation silicon crystal nano surface treatment agent comprises the following steps: mixing and stirring composite modified silicate, polymer solution, metal oxide nano particle dispersion, defoamer and water uniformly to obtain the agent.

[0089] The invention discloses an application of a highly efficient anti-oxidation silicon crystal nano-surface treatment agent for the protection of photovoltaic glass.

[0090] Example 2

[0091] Example 2 provides a high-efficiency anti-oxidation silicon crystal nano-surface treatment agent, which comprises, by weight, 42 parts of composite modified silicate, 10 parts of polymer solution, 12 parts of metal oxide nanoparticle dispersion, 2 parts of defoaming agent, and 40 parts of water;

[0092] The composite modified silicate is a silicate coated with modified particles; the silicate includes alkali metal silicate and layered structure silicate;

[0093] The preparation method of the modified particles comprises the following steps: mixing the particles in ethanol for 40 minutes, then adding N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and aluminum acetate, and reacting at 65° C. for 45 minutes to obtain the modified particles;

[0094] The particles include graphene, carbon nanotubes, and rare earth oxides in a mass ratio of 15:4:1;

[0095] The graphene has a wrinkled structure and a thickness of 2±1 nm; it was purchased from Nanjing Jicang Nanotechnology Co., Ltd., model: JCVDG-2-30.

[0096] The carbon nanotubes are a mixture of multi-walled carbon nanotubes with a diameter of 11.5±3.5 nm and multi-walled carbon nanotubes with a diameter of 40±10 nm, with a mass ratio of 8:5; they are purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., and the models are: XFM10 and XFM28 respectively.

[0097] The rare earth oxides are spherical lanthanum oxide with a particle size of 40 nm and irregular yttrium oxide with a particle size of 1 μm, with a mass ratio of 2:1; they are purchased from Yijin New Materials.

[0098] The mass ratio of the particles, ethanol, N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and aluminum acetate is 20:150:0.4:0.3.

[0099] The preparation method of the composite modified silicate comprises the following steps: dispersing the silicate in a 70 vol% ethanol aqueous solution by ultrasonication, adding the modified particles under stirring, reacting at 60° C. for 7 hours, and then drying to obtain the composite modified silicate;

[0100] The mass ratio of the silicate, the ethanol aqueous solution and the modified particles is 8:100:4.

[0101] The mass ratio of the alkali metal silicate to the layered silicate is 2:1.

[0102] The alkali metal silicates are potassium silicate and sodium silicate.

[0103] The mass ratio of the potassium silicate to the sodium silicate is 12:5.

[0104] The layered silicate is talcum powder and mica powder, with a mass ratio of 1:1.

[0105] The mica powder has an aspect ratio of 80 and a D50 of 12±2 μm and is purchased from Guangdong Yongfeng Chemical Co., Ltd. Model: ZR-C2.

[0106] The talcum powder D50 is 6.1±0.1 μm and is customized from Quanzhou Yiluoke New Materials Co., Ltd.

[0107] The polymer solution is a polyvinyl alcohol aqueous solution.

[0108] The polyvinyl alcohol is polyvinyl alcohol PVA100-60.

[0109] The polyvinyl alcohol PVA100-60 has a degree of alcoholysis of 95±1 mol% and a viscosity of 25±3 mPa.s and was purchased from Guangzhou Jingyi New Materials Co., Ltd., model: 094-27.

[0110] The polyvinyl alcohol aqueous solution consists of polyvinyl alcohol and water in a mass ratio of 12:1000.

[0111] The metal oxide nanoparticles in the metal oxide nanoparticle dispersion are a combination of titanium dioxide and zinc oxide.

[0112] The mass ratio of titanium dioxide to zinc oxide is 18:12.

[0113] The titanium dioxide is mixed crystal titanium dioxide.

[0114] The mixed crystal titanium dioxide has a particle size of 20 nm and is purchased from Brofos Nanotechnology (Ningbo) Co., Ltd., model: Brofos-TiO2-RJ20.

[0115] The zinc oxide has a particle size of 50 nm and is purchased from Brofos Nanotechnology (Ningbo) Co., Ltd., model: Brofos-ZnO-50.

[0116] The preparation method of the metal oxide nanoparticle dispersion comprises the following steps: mixing the metal oxide nanoparticles, a polymer dispersant and water at a mass ratio of 25:2:100 and performing ultrasonic dispersion to uniformly obtain the dispersion.

[0117] The polymer dispersant is a high molecular weight copolymer containing pigment affinity groups, model: BYK-9077.

[0118] The defoamer is an organosilicon defoamer, model: BYK-024.

[0119] A method for preparing a high-efficiency anti-oxidation silicon crystal nano surface treatment agent comprises the following steps: mixing and stirring composite modified silicate, polymer solution, metal oxide nano particle dispersion, defoamer and water uniformly to obtain the agent.

[0120] The invention discloses an application of a highly efficient anti-oxidation silicon crystal nano-surface treatment agent for the protection of photovoltaic glass.

[0121] Example 3

[0122] Example 3 provides a high-efficiency antioxidant silicon crystal nano-surface treatment agent, which comprises, by mass, 60 parts of composite modified silicate, 15 parts of polymer solution, 18 parts of metal oxide nanoparticle dispersion, 3 parts of defoaming agent, and 60 parts of water;

[0123] The composite modified silicate is a silicate coated with modified particles; the silicate includes alkali metal silicate and layered structure silicate;

[0124] The preparation method of the modified particles comprises the following steps: mixing the particles in ethanol for 40 minutes, then adding N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and aluminum acetate, and reacting at 65° C. for 45 minutes to obtain the modified particles;

[0125] The particles include graphene, carbon nanotubes, and rare earth oxides in a mass ratio of 15:4:1;

[0126] The graphene has a wrinkled structure and a thickness of 2±1 nm; it was purchased from Nanjing Jicang Nanotechnology Co., Ltd., model: JCVDG-2-30.

[0127] The multi-walled carbon nanotubes with a carbon nanotube diameter of 11.5±3.5 nm and the multi-walled carbon nanotubes with a carbon nanotube diameter of 40±10 nm are compounded at a mass ratio of 8:5; they are purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., and the models are: XFM10 and XFM28 respectively.

[0128] The rare earth oxides are spherical lanthanum oxide with a particle size of 40 nm and irregular yttrium oxide with a particle size of 1 μm, with a mass ratio of 2:1; they are purchased from Yijin New Materials.

[0129] The mass ratio of the particles, ethanol, N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and aluminum acetate is 20:150:0.4:0.3.

[0130] The preparation method of the composite modified silicate comprises the following steps: dispersing the silicate in a 70 vol% ethanol aqueous solution by ultrasonication, adding the modified particles under stirring, reacting at 60° C. for 7 hours and then drying to obtain the composite modified silicate;

[0131] The mass ratio of the silicate, the ethanol aqueous solution and the modified particles is 8:100:4.

[0132] The mass ratio of the alkali metal silicate to the layered silicate is 2:1.

[0133] The alkali metal silicates are potassium silicate and sodium silicate.

[0134] The mass ratio of the potassium silicate to the sodium silicate is 12:5.

[0135] The layered silicate is talcum powder and mica powder, with a mass ratio of 1:1.

[0136] The mica powder has an aspect ratio of 80 and a D50 of 12±2 μm and is purchased from Guangdong Yongfeng Chemical Co., Ltd. Model: ZR-C2.

[0137] The talcum powder D50 is 6.1±0.1 μm and is customized from Quanzhou Yiluoke New Materials Co., Ltd.

[0138] The polymer solution is a polyvinyl alcohol aqueous solution.

[0139] The polyvinyl alcohol is polyvinyl alcohol PVA100-60.

[0140] The polyvinyl alcohol PVA100-60 has a degree of alcoholysis of 95±1 mol% and a viscosity of 25±3 mPa.s and was purchased from Guangzhou Jingyi New Materials Co., Ltd., model: 094-27.

[0141] The polyvinyl alcohol aqueous solution consists of polyvinyl alcohol and water in a mass ratio of 12:1000.

[0142] The metal oxide nanoparticles in the metal oxide nanoparticle dispersion are a combination of titanium dioxide and zinc oxide.

[0143] The mass ratio of titanium dioxide to zinc oxide is 18:12.

[0144] The titanium dioxide is mixed crystal titanium dioxide.

[0145] The mixed crystal titanium dioxide has a particle size of 20 nm and is purchased from Brofos Nanotechnology (Ningbo) Co., Ltd., model: Brofos-TiO2-RJ20.

[0146] The zinc oxide has a particle size of 50 nm and is purchased from Brofos Nanotechnology (Ningbo) Co., Ltd. Model: Brofos-Z n O-50.

[0147] The preparation method of the metal oxide nanoparticle dispersion comprises the following steps: mixing the metal oxide nanoparticles, a polymer dispersant and water at a mass ratio of 25:2:100 and performing ultrasonic dispersion to uniformly obtain the dispersion.

[0148] The polymer dispersant is a high molecular weight copolymer containing pigment affinity groups, model: BYK-9077.

[0149] The defoamer is an organosilicon defoamer, model: BYK-024.

[0150] A method for preparing a high-efficiency anti-oxidation silicon crystal nano surface treatment agent comprises the following steps: mixing and stirring composite modified silicate, polymer solution, metal oxide nano particle dispersion, defoamer and water uniformly to obtain the agent.

[0151] The invention discloses an application of a highly efficient anti-oxidation silicon crystal nano-surface treatment agent for the protection of photovoltaic glass.

[0152] Comparative Example 1

[0153] Comparative Example 1 provides a high-efficiency antioxidant silicon crystal nano-surface treatment agent, a preparation method and an application thereof. Its specific implementation manner is the same as that of Example 1, except that the high-efficiency antioxidant silicon crystal nano-surface treatment agent comprises, by mass, 32 parts of silicate, 16 parts of modified particles, 12 parts of polymer solution, 15 parts of metal oxide nanoparticle dispersion, 2 parts of defoaming agent and 50 parts of water.

[0154] Comparative Example 2

[0155] Comparative Example 2 provides a high-efficiency antioxidant silicon crystal nano-surface treatment agent and its preparation method and application. Its specific implementation method is the same as Example 1, except that the preparation method of the modified particles includes the following steps: supermixing and stirring the particles in ethanol for 40 minutes, then adding N-β (aminoethyl) -γ-aminopropyltrimethoxysilane, and reacting at 65°C for 45 minutes to obtain.

[0156] The mass ratio of the particles, ethanol, N-β (aminoethyl)-γ-aminopropyltrimethoxysilane and aluminum acetate is 20:150:0.4.

[0157] Comparative Example 3

[0158] Comparative Example 3 provides a highly efficient antioxidant silicon crystal nano-surface treatment agent, a preparation method and an application thereof, and its specific implementation manner is the same as that of Example 1, except that the particles include graphene, carbon nanotubes and rare earth oxides in a mass ratio of 25:1:3.

[0159] Comparative Example 4

[0160] Comparative Example 4 provides a high-efficiency antioxidant silicon crystal nano-surface treatment agent, a preparation method and an application thereof, and its specific implementation manner is the same as that of Example 1, except that the graphene is industrial-grade single-layer graphene purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., model: XFSG05.

[0161] Comparative Example 5

[0162] Comparative Example 5 provides a high-efficiency antioxidant silicon crystal nano-surface treatment agent, a preparation method and an application. Its specific implementation method is the same as Example 1, except that the multi-walled carbon nanotubes with a diameter of 40±10nm are replaced with multi-walled carbon nanotubes with a diameter of >50nm, which are purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., model: XFM34.

[0163] Comparative Example 6

[0164] Comparative Example 6 provides a highly efficient antioxidant silicon crystal nano-surface treatment agent, a preparation method and an application thereof, and its specific implementation manner is the same as that of Example 1, except that the mass ratio of potassium silicate to sodium silicate is 20:1.

[0165] Comparative Example 7

[0166] Comparative Example 7 provides a high-efficiency antioxidant silicon crystal nano-surface treatment agent, a preparation method and an application. Its specific implementation method is the same as Example 1, except that the mica powder has an aspect ratio of 100 and a D50 of 7±2 μm. It is purchased from Guangdong Yongfeng Chemical Co., Ltd., model: ZR-C3.

[0167] Comparative Example 8

[0168] Comparative Example 8 provides a high-efficiency antioxidant silicon crystal nano-surface treatment agent, a preparation method and an application. Its specific implementation method is the same as Example 1, except that the polyvinyl alcohol PVA100-60 has a degree of alcoholysis of 86±1 mol% and a viscosity of 3.8±0.4 mPa.s, and is purchased from Guangzhou Jingyi New Materials Co., Ltd., model: 086-03.

[0169] Comparative Example 9

[0170] Comparative Example 9 provides a highly efficient antioxidant silicon crystal nano-surface treatment agent, a preparation method and an application thereof, and its specific implementation manner is the same as that of Example 1, except that the mass portion of the composite modified silicate is 40 parts, and the mass portion of the polymer is 20 parts.

[0171] Comparative Example 10

[0172] Comparative Example 10 provides a high-efficiency antioxidant silicon crystal nano-surface treatment agent, a preparation method and an application. Its specific implementation method is the same as Example 1, except that the titanium dioxide is rutile titanium dioxide with a particle size of 20 nm, purchased from Brofos Nano Technology (Ningbo) Co., Ltd., model: Brofos-TiO2-J20.

[0173] Comparative Example 11

[0174] Comparative Example 11 provides a highly efficient antioxidant silicon crystal nano-surface treatment agent, a preparation method and an application thereof, and its specific implementation manner is the same as that of Example 1, except that the mass ratio of titanium dioxide to zinc oxide is 25:5.

[0175] Performance test: The surface treatment agent prepared in Examples 1-3 and Comparative Example 1.11 was sprayed on the surface of photovoltaic glass, and dried at room temperature to form a 1 μm film layer, and the film layer was tested for the items shown in Table 1;

[0176] Solar effective transmittance: tested using a UV-visible-near-infrared spectrometer from Hengao Instruments after 4 months of outdoor exposure; Solar effective transmittance refers to the average solar effective transmittance in the wavelength range of 340-1500nm.

[0177] Water contact angle: tested using a contact angle meter.

[0178] Resistivity: Tested using a surface resistance tester.

[0179] Wet and frost resistance: at a relative humidity of 85% ± 5%, the maximum temperature is 85℃ ± 2℃ and drops to -40℃ ± 2℃, and the number of cycles is 20. After the test, the average value of the effective transmittance of sunlight should be attenuated by no more than 1%, and the film is considered qualified if there is no obvious shedding, peeling, or wrinkling.

[0180] Resistance to moisture and heat: At a relative temperature of 85℃±2℃ and a relative humidity of 85%±2%, the test time is 2000 hours. The average value of the effective transmittance of sunlight should be attenuated by no more than 1%, and the film should be considered qualified if there is no obvious shedding, peeling or wrinkling.

[0181] Neutral salt spray resistance: at 35±2℃, using 5% salt water, the test time is 96h. After 96 hours of salt spray test, the average value of the effective transmittance of sunlight should be attenuated by no more than 1%, and there should be no obvious shedding, peeling or wrinkling of the film, which is considered qualified.

[0182] The test results are shown in Table 1 and Table 2:

[0183] Table 1

[0184]

[0185] Table 2

[0186]

[0187]

[0188] It can be seen from Tables 1 and 2 above that in Comparative Example 1, due to the direct mixing of silicate and graphene, the water contact angle of the surface modifier obtained is significantly increased, the effective sunlight transmittance of the photovoltaic glass is relatively low, and the moisture and frost resistance and neutral salt spray resistance are both unqualified.

[0189] Comparative Examples 2-5 respectively changed the preparation method of the modified particles, the ratio between the particles, the structure of the graphene and the particle size of the carbon nanotubes, and the obtained surface modifiers had relatively poor solar effective transmittance, salt spray resistance and hydrophilicity.

[0190] In Comparative Examples 6-7, the ratio of alkali metal silicates and the diameter-to-thickness ratio of mica powder were changed, and the surface modifier obtained had poor resistance to moisture and frost and moisture and heat.

[0191] Comparative Examples 8-9 change the alcoholysis degree of polyvinyl alcohol and the mass ratio of the composite modified silicate and the polymer, and the obtained surface modifier cannot achieve super hydrophilicity and has poor moisture and freeze resistance.

[0192] In Comparative Examples 10-11, the crystal form of titanium dioxide and the mass ratio of titanium dioxide to zinc oxide were changed, and the light transmittance of the photovoltaic glass was poor.

[0193] The above description is only a specific embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent transformation made by the present invention, or directly or indirectly applied in other related technical fields, is also included in the patent protection scope of the present invention.

Claims

1. A highly efficient anti-oxidation silicon crystal nano-surface treatment agent, characterized in that: The composition comprises, by weight, 50 parts of a composite modified silicate, 12 parts of a polymer solution, 15 parts of a metal oxide nanoparticle dispersion, 2 parts of a defoaming agent, and 50 parts of water; The composite modified silicate is a silicate coated with modified particles; the silicate includes alkali metal silicate and layered structure silicate; The preparation method of the modified particles comprises the following steps: mixing the particles in ethanol for 40 minutes, then adding N-β (aminoethyl) -γ-aminopropyltrimethoxysilane and aluminum acetate, and reacting at 65° C. for 45 minutes to obtain the modified particles; The particles include graphene, carbon nanotubes, and rare earth oxides in a mass ratio of 15:4:1; The graphene has a wrinkled structure and a thickness of 2±1 nm; The carbon nanotubes are a composite of multi-walled carbon nanotubes with a diameter of 11.5±3.5 nm and multi-walled carbon nanotubes with a diameter of 40±10 nm, with a mass ratio of 8:5; The rare earth oxides are spherical lanthanum oxide with a particle size of 40 nm and irregular yttrium oxide with a particle size of 1 μm, with a mass ratio of 2:1; The mass ratio of the particles, ethanol, N-β (aminoethyl)-γ-aminopropyltrimethoxysilane and aluminum acetate is 20:150:0.4:0.3; The preparation method of the composite modified silicate comprises the following steps: dispersing the silicate in a 70 vol% ethanol aqueous solution by ultrasonication, adding the modified particles under stirring, reacting at 60° C. for 7 hours, and then drying to obtain the composite modified silicate; The mass ratio of the silicate, ethanol aqueous solution and modified particles is 8:100:4; The mass ratio of the alkali metal silicate to the layered silicate is 2:1; The alkali metal silicates are potassium silicate and sodium silicate; The mass ratio of potassium silicate to sodium silicate is 12:5; The layered silicate is talc powder and mica powder, with a mass ratio of 1:1; The mica powder has an aspect ratio of 80 and a D50 of 12±2 μm; The talcum powder D50 is 6.1±0.1 μm; The polymer solution is a polyvinyl alcohol aqueous solution; The polyvinyl alcohol is polyvinyl alcohol PVA100-60; The polyvinyl alcohol PVA100-60 has a degree of alcoholysis of 95±1 mol% and a viscosity of 25±3 mPa.s; The polyvinyl alcohol aqueous solution is composed of polyvinyl alcohol and water in a mass ratio of 12:1000; The metal oxide nanoparticles in the metal oxide nanoparticle dispersion are a combination of titanium dioxide and zinc oxide; The mass ratio of titanium dioxide to zinc oxide is 18:12; The titanium dioxide is mixed crystal titanium dioxide; The particle size of the mixed crystal titanium dioxide is 20 nm; The particle size of the zinc oxide is 50 nm; The preparation method of the metal oxide nanoparticle dispersion comprises the following steps: mixing metal oxide nanoparticles, a polymer dispersant and water at a mass ratio of 25:2:100 and performing ultrasonic dispersion to uniformly obtain the dispersion; The polymer dispersant is a high molecular weight copolymer containing pigment affinity groups; The defoamer is an organosilicon defoamer.

2. A method for preparing a high-efficiency anti-oxidation silicon crystal nano-surface treatment agent according to claim 1, characterized in that: The method comprises the following steps: mixing and stirring the composite modified silicate, polymer solution, metal oxide nanoparticle dispersion, defoamer and water evenly.

3. An application of the high-efficiency anti-oxidation silicon crystal nano-surface treatment agent according to claim 1, characterized in that: Used for protection of photovoltaic glass.