Epoxy resin composition for adhesive and preparation method thereof, adhesive

By using a combination of phthalic anhydride polyester polyol and an amine-based curing agent in epoxy resin adhesive, the toughness and viscosity problems of epoxy resin adhesive are solved, efficient toughening modification is achieved, and the performance and economicality of the adhesive are improved.

CN118240518BActive Publication Date: 2024-11-12HUIZHOU JIADINGGU CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410502722.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2024-11-12
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

The existing epoxy resin adhesives have problems such as brittle quality, poor toughness, poor heat resistance and poor impact resistance. The existing toughening agents have problems such as high viscosity, high cost or difficult processing in improving toughness.

Method used

Using phthalic anhydride polyester polyol as a toughening agent, a epoxy resin composition with good compatibility is formed by combining it with bisphenol A-type epoxy resin and an amine-based curing agent, and an ester bond of phthalic anhydride polyester polyol is used. and aromatic structures improve toughness and optimize viscosity and curing properties through specific combination distribution ratios and process treatments.

Benefits of technology

The toughness of the epoxy resin composition is improved, the viscosity and cost are reduced, the compatibility with the epoxy resin is improved, the tensile breaking energy and impact resistance of the adhesive are enhanced, and the thermal deformation temperature is maintained at a high level. and low viscosity characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118240518B_ABST
    Figure CN118240518B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of adhesives, and in particular to an epoxy resin composition for adhesives, a preparation method thereof, and an adhesive. The epoxy resin composition for adhesives provided by the present invention comprises component A and component B; in parts by weight, the component A comprises the following components: 100 parts of epoxy resin, 1-25 parts of toughening agent; component B is an amine curing agent; wherein the toughening agent is phthalic anhydride polyester polyol. The epoxy resin composition of the present invention can improve elongation at break, tensile fracture energy, has a high glass transition temperature Tg, and has good comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesives, and in particular to an epoxy resin composition for adhesives, a preparation method thereof, and an adhesive. Background Art

[0002] Epoxy resin (EP) is a general term for a class of polymers containing more than two epoxy groups in the molecule. It is a polycondensation product of epichlorohydrin and bisphenol A or polyols. Due to the chemical activity of the epoxy group, it can be opened with a variety of compounds containing active hydrogen. After curing, it presents a highly cross-linked three-dimensional network structure with excellent bonding strength, dielectric properties, corrosion resistance, mechanical properties and low curing shrinkage. As an excellent matrix material, it is widely used in coatings, adhesives, insulation materials, national defense, military industry, aerospace, construction, light industry and other fields. However, its cured product has the disadvantages of being brittle, poor toughness, poor heat resistance and poor impact resistance, which restrict its application. Therefore, it is necessary to toughen the epoxy resin, especially when used as an adhesive, it is necessary to undergo appropriate toughening modification so that it meets the actual technical and cost requirements.

[0003] Generally, toughening modification is to add toughening agents to epoxy resins to achieve the purpose of toughening through various toughening mechanisms. Relevant technicians have conducted a lot of research on the toughening modification of epoxy resins. Commonly used toughening agents are: reactive liquid nitrile rubber, such as carboxyl-terminated nitrile rubber (CTBN) and amine-terminated nitrile rubber (ABTN); thermoplastic resins, such as polyvinyl butyral (PVB); blocked isocyanate or epoxy-modified polyurethane toughening agents; polyether polyols; polyester polyols.

[0004] However, the existing toughening agents still have the following shortcomings: when reactive liquid nitrile rubber is used with a curing agent at room temperature, CTBN and an excess of epoxy resin need to be reacted in advance to obtain a modified epoxy resin, and the viscosity is very high and the price is high; ATBN has poor compatibility with some high-polarity curing agents, and the viscosity is also very high and the price is high; PVB has a large molecular weight, so the viscosity increases a lot after it is added to the epoxy resin, which in some cases makes processing difficult and is not conducive to increasing the amount of filler added; blocked isocyanate or epoxy-modified polyurethane toughening agents also have a large viscosity and are mostly used to increase flexibility. Properties; Polyether polyols, Chinese invention patent application CN102884100A mentions that although low molecular weight polyether polyols have low viscosity and low cost, they will greatly reduce the Tg of the cured product and are often used in heat-cured acid anhydride systems; Polyester polyols, Chinese invention patent application CN103396536A uses aromatic tricarboxylic anhydride or tetracarboxylic anhydride and polyols to react to obtain polyester polyol toughening agents. Although the modified cured product maintains a high heat deformation temperature and good impact resistance, its viscosity at 25°C is greater than 5000 centipoise, and it is an acid anhydride system for heat curing.

[0005] Therefore, there is an urgent need to find a new way to improve the defects of epoxy resin cured products, such as high brittleness, poor toughness and poor impact resistance. Summary of the invention

[0006] In order to solve the above technical problems existing in the prior art, the present invention provides an epoxy resin composition for adhesive and a preparation method thereof, and an adhesive.

[0007] The technical solution of the present invention to solve the above technical problems is as follows:

[0008] The first aspect of the present invention provides an epoxy resin composition for adhesive, characterized in that it comprises component A and component B;

[0009] In parts by weight, the component A comprises the following components: 100 parts of epoxy resin and 1-25 parts of toughening agent;

[0010] The B component is an amine curing agent;

[0011] Wherein, the toughening agent is phthalic anhydride polyester polyol.

[0012] On the basis of the above technical solution, the present invention can also make the following improvements:

[0013] Furthermore, the phthalic anhydride polyester polyol is obtained by polycondensation of phthalic anhydride and polyol, and the polyol is selected from small molecule polyol or small molecular weight polyether polyol.

[0014] Furthermore, the small molecule polyol is selected from any one or more of ethylene glycol, 1,2-propylene glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, trimethylolpropane, glycerol, and low molecular weight polyethylene glycol, and the low molecular weight polyether polyol is selected from polyethylene glycol or polypropylene glycol.

[0015] Furthermore, the amine curing agent is a modified alicyclic amine or a modified fatty amine.

[0016] Furthermore, the modified fatty amine is any one of the addition product of polyethylene polyamine and aromatic glycidyl ether, Mannich base (phenalkamine) or polyether amine, preferably an addition product obtained by the reaction of diethylenetriamine (DETA) and phenyl glycidyl ether (PGE) or o-toluene glycidyl ether (CGE), and further preferably a polyethylene polyamine-modified JH-5413-3M curing agent to improve compatibility with epoxy resin.

[0017] Mannich base is a phenolic amine type curing agent, which is obtained by the reaction of phenol, aldehyde and amine. The type of phenol generally used is phenol, and nonylphenol, o-cresol, p-tert-butylphenol, and cardanol can also be used; the amine usually uses ethyleneamine, such as ethylenediamine (EDA), diethylenetriamine (DETA), triethylenetetramine (TETA), and other amines can also be used, such as meta-xylylenediamine (MXDA) and isophoronediamine (IPDA); the aldehyde usually uses formaldehyde, and other aldehydes can also be used.

[0018] Furthermore, the modified alicyclic amine is any one of an adduct of isophoronediamine and bisphenol A epoxy resin, an adduct of diaminodicyclohexylmethane (PACM) and bisphenol A epoxy resin, an adduct of aminoethylpiperazine and aromatic glycidyl ether, and an adduct of aminoethylpiperazine and bisphenol A epoxy resin.

[0019] Furthermore, the phthalic anhydride polyester polyol is STEPANOL PDP-70.

[0020] Furthermore, the epoxy resin is a bisphenol A epoxy resin, preferably NPEL-128.

[0021] The beneficial effect of adopting the above-mentioned further technical scheme is that both the structures of phthalic anhydride polyester polyol and bisphenol A epoxy resin contain aromatic structural groups. According to the principle of similar compatibility, phthalic anhydride polyester polyol and bisphenol A epoxy resin have good compatibility, and the ester bond contained in the structure of phthalic anhydride polyester polyol has high polarity, which is also conducive to improving its compatibility with epoxy resin.

[0022] Furthermore, the component A also includes 0-20 parts of a diluent to reduce viscosity.

[0023] Furthermore, the weight ratio of component A to component B is 100:25-50.

[0024] The weight ratio of component A to component B is calculated based on the epoxy equivalent of component A and the active hydrogen equivalent of component B and is obtained through experimental optimization.

[0025] The second aspect of the present invention provides a method for preparing the above-mentioned epoxy resin composition for adhesive, comprising the following steps:

[0026] (1) heating the epoxy resin and toughening agent to 60-80° C. according to weight proportions and stirring and mixing for 30-60 minutes, and then cooling to room temperature to obtain component A for standby use;

[0027] (2) At room temperature, the component A and the component B are uniformly mixed and cured to obtain the epoxy resin composition for adhesive.

[0028] Another aspect of the present invention provides an adhesive, comprising the epoxy resin composition for adhesive.

[0029] Compared with the prior art, the present invention has the following technical effects:

[0030] The present invention selects phthalic anhydride polyester polyol as the toughening agent of epoxy resin, which contains a rigid benzene ring structure and a polar ester bond on the main chain, and also contains a flexible polyol segment, has a relatively low viscosity of 1000-5000 centipoise at 25°C, has good compatibility with epoxy resin and amine curing agent, low viscosity, and high cost performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The stress-strain curves of the tensile strength test of various embodiments and comparative examples of the present invention are shown (0 PHR: comparative example, 5 PHR: embodiment 1, 10 PHR: embodiment 2, 15 PHR: embodiment 3). DETAILED DESCRIPTION

[0032] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may extend based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0033] Example 1

[0034] Preparation process:

[0035] (1) Weigh 100 g of NPEL-128 and 5 g of STEPANOL PDP-70, heat to 60° C. and stir for 30 minutes, then cool to room temperature to obtain epoxy component A for later use;

[0036] (2) Use modified fatty amine curing agent JH-5413-3M as component B, and the dosage is 1 / 3 of NPEL-128;

[0037] (3) At room temperature, component A and component B were mixed evenly, and then cured at 40° C. for 24 hours to obtain the epoxy resin composition of Example 1.

[0038] Example 2

[0039] The added amount of STEPANOL PDP-70 is 10 g, and the rest is the same as in Example 1.

[0040] Example 3

[0041] The added amount of STEPANOL PDP-70 is 15 g, and the rest is the same as in Example 1.

[0042] Comparative Example

[0043] The phthalic anhydride polyester polyol was not added, and the rest was the same as in Example 1.

[0044] Note: Examples 1-3 and the comparative example are all cured at 40°C for 24 hours. The curing effect of this curing condition is equivalent to the curing effect of curing for seven days at room temperature. The present invention shortens the curing time by increasing the curing temperature.

[0045] The performance of the epoxy resin compositions of Examples 1-3 and Comparative Examples was tested using the following method:

[0046] The tensile properties were tested in accordance with GB / T 2567-2008 "Test methods for properties of resin castings", and the electronic tensile testing machine used was LLOYD EZ20 material testing machine;

[0047] Test the shear strength according to GB / T 7124-2008 "Determination of tensile shear strength of adhesives (rigid material to rigid material)";

[0048] Tg was tested using a DSC instrument; a heating rate of 10°C / min was used, and the scanning range was 40-250°C for curing, then the temperature was lowered to 25°C and then scanned at a heating rate of 10°C / min until it reached 150°C, and the midpoint method was used for measurement.

[0049] Specific performance data are shown in Table 1.

[0050] Table 1 Performance data of various epoxy resin compositions

[0051]

[0052]

[0053] Note: Breaking energy: The stress-strain curve of the tensile strength test (such as Figure 1 The integral area of ​​the tensile spline fracture area is divided by the tensile spline fracture area (the tensile spline fracture area is 1.28*0.33cm 2 ).

[0054] It can be seen from Table 1 that when the toughening agent content increases from 0 to 15 parts by weight, the tensile fracture energy increases from 4.41 J / cm 2 Increased to 7.15 J / cm 2 , increased by 62.1%; the elongation at break increased from 2.62% to 4.13%; and the glass transition temperature Tg only slightly decreased from 70.4°C to 64.41°C, and the decrease in tensile strength was not very high and maintained at a high level, indicating that this toughening agent has a good toughening effect and low viscosity (2000 centipoise, 25°C).

[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. An epoxy resin composition for adhesive, It is characterized in that It includes component A and component B; In parts by weight, the component A comprises the following components: 100 parts of epoxy resin and 1-25 parts of toughening agent; The component B is an amine curing agent; Wherein, the toughening agent is phthalic anhydride polyester polyol; The amine curing agent is JH-5413-3M curing agent modified with polyethylene polyamine, the phthalic anhydride polyester polyol is STEPANOLPDP-70, the epoxy resin is NPEL-128, and the weight ratio of component A to component B is 100:25-50.

2. The epoxy resin composition for adhesive according to claim 1, It is characterized in that The A component also includes 0-20 parts of a diluent.

3. A method for preparing the epoxy resin composition for adhesive according to claim 1 or 2, It is characterized in that The following steps are involved: (1) According to the weight ratio, the epoxy resin and toughening agent are heated to 60-80° C. and stirred for 30-60 minutes, and then allowed to stand and cool to room temperature to obtain component A for standby use; (2) At room temperature, the component A and the component B are uniformly mixed and cured to obtain the epoxy resin composition for adhesive.

4. An adhesive, It is characterized in that The invention comprises the epoxy resin composition for adhesive according to claim 1 or 2.