A flexible photovoltaic backsheet and a manufacturing method thereof

Through the combination of epoxy resin and glass fiber and hot-pressing composite technology, a highly rigid and flexible photovoltaic backsheet is prepared, which solves the problem of insufficient rigidity of existing photovoltaic backsheet materials and achieves effective support and protection for cells. And it has good production applicability and economic benefits.

CN118248787BActive Publication Date: 2024-10-15ZHONGKE WEIHE TECH (ZHAOQING) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410389237.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-02
Publication Date
2024-10-15
Estimated Expiration
2044-04-02

AI Technical Summary

Technical Problem

Existing photovoltaic backsheet materials are not rigid enough to effectively support and protect solar cells, and traditional thermoplastic packaging materials are limited in the installation environment.

Method used

The epoxy resin glass fiber prepreg is prepared by combining epoxy resin and glass fiber, and is combined with the polyvinyl chloride board through hot pressing composite technology to form a flexible photovoltaic backsheet, which is well combined and has high rigidity and flexibility.

Benefits of technology

It achieves effective support and protection for the battery cells, and at the same time has good flexibility, is suitable for industrial mass production, and has good application prospects and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118248787B_ABST
    Figure CN118248787B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of photovoltaic backboards, and more specifically, it relates to a flexible photovoltaic backboard and a method for making the same. The technical solution thereof includes the following steps: S1, obtaining an epoxy resin composition and a glass fiber cloth, uniformly coating the epoxy resin composition on the glass fiber cloth, baking, cooling, obtaining a semi-finished product, and shearing the semi-finished product according to size requirements to obtain an epoxy resin glass fiber semi-cured sheet; S2, obtaining a first polyvinyl chloride board and a second polyvinyl chloride board, using the epoxy resin glass fiber semi-cured sheet as a bonding layer, stacking the bonding layer between the first polyvinyl chloride board and the second polyvinyl chloride board to obtain a stacked composite layer; S3, placing the composite layer in a mold, hot pressing, and obtaining a target product; the epoxy resin composition includes a main epoxy resin, a curing agent, a reaction accelerator, a bonding promoter, and a solvent. The present invention has excellent support and protection effects on battery cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photovoltaic back panels, and more specifically, to a flexible photovoltaic back panel and a manufacturing method thereof. Background Art

[0002] Solar cell modules mainly include backplane, solar cell circuit, encapsulation film and front panel. Among them, the photovoltaic backplane is located on the back of the solar cell panel, which protects and supports the cells. It has reliable insulation, water resistance and aging resistance, and is an important encapsulation structure in photovoltaic modules.

[0003] Early solar photovoltaic cells were encapsulated in glass, which had the problems of being heavy and not resistant to impact, and thus limited their installation environment. Some manufacturers used thermoplastics as encapsulation materials to solve the problem of heavy weight and not resistant to impact of photovoltaic back panels, but the use of thermoplastics still had the following defects: the photovoltaic back panel was not rigid enough and was too soft, making it difficult to support and protect the battery cells.

[0004] A Chinese patent document with publication number CN100365831 C discloses a packaging method for large-area lightweight solar cells, a lightweight crystalline silicon solar cell module using an FR-4 epoxy glass fiber substrate as a backplane, but the FR-4 epoxy glass fiber substrate is a rigid material and still lacks flexibility, which makes the installation environment of the module subject to certain restrictions. Summary of the invention

[0005] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a flexible photovoltaic backplane and a method for manufacturing the same, which can support the solar cells while being flexible and providing better protection for the solar cells.

[0006] The above technical objectives of the present invention are achieved through the following technical solutions: A method for manufacturing a flexible photovoltaic backsheet, comprising the following steps:

[0007] S1, obtaining an epoxy resin composition and a glass fiber cloth, uniformly coating the epoxy resin composition on the glass fiber cloth, baking, cooling, obtaining a semi-finished product, and cutting the semi-finished product according to size requirements to obtain an epoxy resin glass fiber prepreg;

[0008] S2, obtaining a first polyvinyl chloride board and a second polyvinyl chloride board, using the epoxy resin glass fiber prepreg as a bonding layer, and stacking the bonding layer between the first polyvinyl chloride board and the second polyvinyl chloride board to obtain a stacked composite layer;

[0009] S3, placing the composite layer into a mold, hot pressing, and obtaining a target product;

[0010] The epoxy resin composition comprises a main epoxy resin, a curing agent, a reaction accelerator, a bonding promoter and a solvent, wherein the main epoxy resin comprises at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, o-cresol epoxy resin, bisphenol A novolac epoxy resin, bromine-containing epoxy resin and phosphorus-containing epoxy resin, and the bonding promoter comprises one or more of thermoplastic acrylate, thermoplastic phenoxy resin, liquid rubber, modified nitrile rubber, nitrile rubber modified epoxy resin, polyurethane modified epoxy resin and polyvinyl acetal.

[0011] In one embodiment, the glass fiber cloth is an electronic grade alkali-free glass fiber cloth, and the gram weight of the electronic grade alkali-free glass fiber cloth is 48-220g / m 2 .

[0012] In one embodiment, the curing agent includes one or more of dicyandiamide, phenolic resin, 4,4'-diaminodiphenyl sulfone and acid anhydride.

[0013] In one embodiment, the reaction accelerator includes one or more of 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, organic urea and 2,4,6-tris(dimethylaminomethyl)phenol.

[0014] In one embodiment, the solvent includes one or more of acetone, butanone, ethylene glycol monomethyl ether, propylene glycol methyl ether and N,N-dimethylformamide.

[0015] In one of the embodiments, the epoxy resin glass fiber prepreg has a resin content of 30-70%.

[0016] In one embodiment, the epoxy resin composition further comprises a functional auxiliary agent, and the functional auxiliary agent comprises one or more of a flame retardant, a pigment, an inorganic filler, an antioxidant, an ultraviolet absorber or a light stabilizer.

[0017] In one embodiment, the flame retardant includes one or more of tetrabromobisphenol A, organic phosphorus, melamine phosphate, melamine cyanurate, aluminum hydroxide and magnesium hydroxide.

[0018] In one of the embodiments, in S2, a plurality of epoxy resin glass fiber prepreg sheets are stacked in the bonding layer.

[0019] A flexible photovoltaic back panel is prepared by the manufacturing method of the flexible photovoltaic back panel.

[0020] The above-mentioned flexible photovoltaic backsheet and its manufacturing method have the following beneficial effects:

[0021] First, by combining the epoxy resin composition with glass fiber, an epoxy resin glass fiber semi-cured sheet with high bonding strength and high rigidity is prepared, and the epoxy resin glass fiber semi-cured sheet is further hot-pressed and composited with a highly flexible polyvinyl chloride board. The obtained flexible photovoltaic backsheet has good bonding, supports the battery cell, and is flexible, so as to better protect the battery cell;

[0022] Second, the manufacturing process is simple and can be implemented on conventional equipment, which is convenient for industrial mass production and has good application prospects and potential economic benefits;

[0023] Third, the design is flexible and can meet different practical application requirements by flexibly adjusting the number of epoxy resin glass fiber semi-cured sheets in the bonding layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a flow chart of the steps of the present invention. DETAILED DESCRIPTION

[0025] The present invention is described in further detail below in conjunction with the embodiments. It should be noted that the embodiments described below are intended to facilitate the understanding of the present invention and do not have any limiting effect on it. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those of ordinary skill in the art to which the present invention belongs. When there is a conflict, the definitions in this specification shall prevail.

[0026] As used herein, the term "prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0027] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0028] When amount, concentration or other value or parameter is expressed as range, preferred range or a series of upper preferred value and lower preferred value limit range, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value and any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when disclosing range "1 to 5", described range should be interpreted as including range "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5" etc. When numerical range is described in this article, unless otherwise stated, the range is intended to include its end value and all integers and fractions within the range.

[0029] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.

[0030] A method for manufacturing a flexible photovoltaic backsheet, such as Figure 1 As shown, the following steps are included:

[0031] S1, obtaining an epoxy resin composition and a glass fiber cloth, uniformly coating the epoxy resin composition on the glass fiber cloth, baking, cooling, obtaining a semi-finished product, and cutting the semi-finished product according to size requirements to obtain an epoxy resin glass fiber prepreg;

[0032] In actual production, the main epoxy resin, curing agent, reaction accelerator, bonding agent and solvent are weighed according to the formula amount to prepare the epoxy resin composition. In addition to uniformly coating the epoxy resin composition on the glass fiber cloth, the glass fiber cloth can also be immersed in the prepared epoxy resin composition and taken out after being completely soaked, so as to obtain the glass fiber cloth uniformly coated with the epoxy resin composition. The glass fiber uniformly coated with the epoxy resin composition is arranged in an oven and baked at a baking temperature of 80-190° C. for 1-15 minutes. The solvent on the glass fiber cloth is removed by baking to obtain a semi-finished product.

[0033] S2, obtaining a first polyvinyl chloride sheet and a second polyvinyl chloride sheet, using an epoxy resin glass fiber prepreg as a bonding layer, and stacking the bonding layer between the first polyvinyl chloride sheet and the second polyvinyl chloride sheet to obtain a stacked composite layer;

[0034] In actual production, both the first polyvinyl chloride board and the second polyvinyl chloride board use polyvinyl chloride with excellent weather resistance, and its flame retardant grade reaches V0 grade. The actual appearance is white, and it will not turn yellow or age even after long-term ultraviolet light exposure. Through the above-mentioned stacking method, the surface layer and the bottom layer of the composite layer are both polyvinyl chloride boards with high flexibility.

[0035] S3, placing the composite layer into a mold, hot pressing, and obtaining the target product;

[0036] In actual production, the hot pressing temperature of S3 is 80-190°C, and the hot pressing time is 0.5-3h. The hot pressing temperature and hot pressing pressure are gradually increased by setting the range value in the vacuum press.

[0037] Among them, in the epoxy resin composition, the addition amount of the main epoxy resin is 80-120 parts, the addition amount of the reaction accelerator is 0.2-2 parts, the addition amount of the bonding promoter is 2-20 parts, the addition amount of the curing agent is affected by the specific selected curing agent type and the main epoxy resin type (so that the molar fraction of the curing agent calculated by active hydrogen equivalent is equivalent to the molar fraction of the epoxy resin calculated by epoxy equivalent), and the addition amount of the solvent is controlled so that the solid content of the epoxy resin composition is 50-70%.

[0038] The main epoxy resin includes at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, o-cresol epoxy resin, bisphenol A novolac epoxy resin, bromine-containing epoxy resin and phosphorus-containing epoxy resin; and the use of bromine-containing epoxy resin and phosphorus-containing epoxy resin helps to improve the flame retardant properties of the photovoltaic backplane, and the use of o-cresol epoxy resin and bisphenol A novolac epoxy resin helps to improve the heat resistance of the photovoltaic backplane.

[0039] The bonding promoter includes one or more of thermoplastic acrylate, thermoplastic phenoxy resin, liquid rubber, modified nitrile rubber, nitrile rubber modified epoxy resin, polyurethane modified epoxy resin and polyvinyl acetal. By adding the bonding promoter, the bonding strength of the polyvinyl chloride board and the epoxy resin glass fiber semi-cured sheet after hot pressing can be strengthened, so that the composite layer after hot pressing is not easy to delaminate.

[0040] The present invention combines an epoxy resin composition with glass fiber to prepare an epoxy resin glass fiber semi-cured sheet with high bonding strength and high rigidity, and further hot-presses the epoxy resin glass fiber semi-cured sheet with a highly flexible polyvinyl chloride plate. The obtained flexible photovoltaic back panel has good bonding, supports the battery cell, and is flexible, so that the battery cell can be better protected. The manufacturing process is simple, and it can be implemented on conventional equipment, which is convenient for industrial mass production, and has good application prospects and potential economic benefits.

[0041] Specifically, the glass fiber cloth is electronic grade alkali-free glass fiber cloth, and the gram weight of the electronic grade alkali-free glass fiber cloth is 48-220g / m 2 In practical applications, glass fiber cloth specifically includes a gram weight of 210g / m 2 7628 electronic grade alkali-free glass fiber cloth, weight 105g / m 2 2116 electronic grade alkali-free glass fiber cloth, weight 78g / m 2 2113 electronic grade alkali-free glass fiber cloth, weight 48g / m 21080 electronic grade alkali-free glass fiber cloth, etc.

[0042] Specifically, the curing agent includes one or more of dicyandiamide, phenolic resin, 4,4'-diaminodiphenyl sulfone and acid anhydride.

[0043] Specifically, the reaction accelerator includes one or more of 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, organic urea and 2,4,6-tris(dimethylaminomethyl)phenol. In actual production, excessively high hot pressing temperature can easily lead to yellowing and aging of polyvinyl chloride sheets. By adding a reaction accelerator to achieve medium-temperature curing, the hot pressing temperature can be reduced.

[0044] Specifically, the solvent includes one or more of acetone, butanone, ethylene glycol monomethyl ether, propylene glycol methyl ether and N,N-dimethylformamide. In actual production, the epoxy resin composition is adjusted to a suitable viscosity by adding a solvent.

[0045] Specifically, the resin content of the epoxy resin glass fiber prepreg is 30-70%.

[0046] Specifically, the epoxy resin composition also includes functional additives, which include one or more of flame retardants, pigments, inorganic fillers, antioxidants, ultraviolet absorbers or light stabilizers. In actual production, the addition of flame retardants can be combined with flame-retardant epoxy resins to achieve a synergistic flame retardant effect; pigments mainly include white titanium dioxide or ground titanium dioxide slurry, and black carbon black or organic dye black; inorganic fillers are used to enhance some properties of flexible photovoltaic backsheets, mainly including silicon micropowder to improve rigidity, talcum powder to improve processing performance, and hollow glass microspheres to reduce density. The amount of functional additives added is determined by actual performance requirements without affecting the bonding strength of the flexible photovoltaic backsheet and the overall performance of the board.

[0047] Further, the flame retardant includes one or more of tetrabromobisphenol A, organic phosphorus, melamine phosphate, melamine cyanurate, aluminum hydroxide and magnesium hydroxide.

[0048] Specifically, in S2, a plurality of epoxy resin glass fiber semi-cured sheets are stacked in the bonding layer, and different practical application requirements can be met by flexibly adjusting the number of epoxy resin glass fiber semi-cured sheets in the bonding layer.

[0049] A flexible photovoltaic back panel is prepared by the manufacturing method of the flexible photovoltaic back panel.

[0050] Example 1

[0051] A flexible photovoltaic backsheet is prepared using the following raw materials: a gram weight of 210 g / m 27628 electronic grade alkali-free glass fiber cloth, bisphenol A epoxy resin, 2-methylimidazole, modified nitrile rubber, dicyandiamide, acetone, and 2 polyvinyl chloride sheets of the same thickness.

[0052] Before making the flexible photovoltaic backsheet, the raw materials are pre-treated:

[0053] (1) Cut the electronic grade alkali-free glass fiber cloth and polyvinyl chloride sheet into the specified size;

[0054] (2) preparing an epoxy resin composition so that the obtained epoxy resin composition meets the following ratio: 100 parts of bisphenol A epoxy resin, 1 part of 2-methylimidazole, 2.5 parts of modified nitrile rubber, and 2 parts of dicyandiamide, and adjusting the mixture by using acetone so that the solid content of the epoxy resin composition is 50-70%.

[0055] After pre-processing the raw materials, the flexible photovoltaic backsheet is made according to the following steps:

[0056] S1, taking an epoxy resin composition and an electronic-grade alkali-free glass fiber cloth, uniformly coating the epoxy resin composition on the electronic-grade alkali-free glass fiber cloth, baking at 190° C. for 3 min, cooling to 25° C. to obtain a semi-finished product, and cutting the semi-finished product according to size requirements to obtain an epoxy resin glass fiber prepreg with a resin content of 30%;

[0057] S2, taking a polyvinyl chloride sheet, using an epoxy resin glass fiber semi-cured sheet as a bonding layer, and stacking the bonding layer between two polyvinyl chloride sheets to obtain a stacked composite layer;

[0058] S3. Place the composite layer obtained in S2 into a mold, hot-press at 110° C. for 1 hour, gradually cool, and demold to obtain a flexible photovoltaic backsheet.

[0059] In this embodiment, a flexible photovoltaic backsheet with a three-layer structure is finally obtained.

[0060] Example 2

[0061] A flexible photovoltaic backsheet is prepared using the following raw materials: a gram weight of 105 g / m 2 2116 electronic grade alkali-free glass fiber cloth, bisphenol A type epoxy resin, bromine-containing epoxy resin, 2-ethyl-4-methylimidazole, liquid rubber, 4,4'-diaminodiphenyl sulfone, ethylene glycol monomethyl ether, tetrabromobisphenol A, and two polyvinyl chloride sheets of the same thickness.

[0062] Before making the flexible photovoltaic backsheet, the raw materials are pre-treated:

[0063] (1) Cut the electronic grade alkali-free glass fiber cloth and polyvinyl chloride sheet into the specified size;

[0064] (2) preparing an epoxy resin composition so that the obtained epoxy resin composition meets the following ratio: 60 parts of bisphenol A epoxy resin, 40 parts of bromine-containing epoxy resin, 2 parts of 2-ethyl-4-methylimidazole, 5 parts of liquid rubber, 15 parts of 4,4'-diaminodiphenyl sulfone, and 20 parts of tetrabromobisphenol A, and adjusting the mixture by using ethylene glycol monomethyl ether so that the solid content of the epoxy resin composition is 50-70%.

[0065] After pre-processing the raw materials, the flexible photovoltaic backsheet is made according to the following steps:

[0066] S1, taking an epoxy resin composition and an electronic-grade alkali-free glass fiber cloth, uniformly coating the epoxy resin composition on the electronic-grade alkali-free glass fiber cloth, baking at 150° C. for 6 min, cooling to 25° C. to obtain a semi-finished product, and cutting the semi-finished product according to size requirements to obtain an epoxy resin glass fiber prepreg with a resin content of 50%;

[0067] S2, taking a polyvinyl chloride sheet, using three epoxy resin glass fiber semi-cured sheets as a bonding layer, and stacking the bonding layer between two polyvinyl chloride sheets to obtain a stacked composite layer;

[0068] S3. Place the composite layer obtained in S2 into a mold, hot-press at 150° C. for 2 h, gradually cool, and demold to obtain a flexible photovoltaic backsheet.

[0069] In this embodiment, a flexible photovoltaic backsheet with a 5-layer structure is finally obtained.

[0070] Example 3

[0071] A flexible photovoltaic backsheet is prepared using the following raw materials: a gram weight of 78 g / m 2 2113 electronic grade alkali-free glass fiber cloth, bisphenol A phenolic epoxy resin, 2-phenylimidazole, thermoplastic acrylate, phenolic resin, butanone, silica powder, and two polyvinyl chloride sheets of the same thickness.

[0072] Before making the flexible photovoltaic backsheet, some raw materials are pre-treated:

[0073] (1) Cut the electronic grade alkali-free glass fiber cloth and polyvinyl chloride sheet into the specified size;

[0074] (2) preparing an epoxy resin composition so that the obtained epoxy resin composition meets the following ratio: 110 parts of bisphenol A novolac epoxy resin, 1.5 parts of 2-phenylimidazole, 7 parts of thermoplastic acrylate, 20 parts of phenolic resin, and 10 parts of silicon powder, and adjusting the mixture by using butanone so that the solid content of the epoxy resin composition is 50-70%.

[0075] After pre-processing the raw materials, the flexible photovoltaic backsheet is made according to the following steps:

[0076] S1, taking an epoxy resin composition and an electronic-grade alkali-free glass fiber cloth, uniformly coating the epoxy resin composition on the electronic-grade alkali-free glass fiber cloth, baking at 80° C. for 15 min, cooling to 25° C. to obtain a semi-finished product, and cutting the semi-finished product according to size requirements to obtain an epoxy resin glass fiber prepreg with a resin content of 70%;

[0077] S2, taking a polyvinyl chloride sheet, using 5 epoxy resin glass fiber semi-cured sheets as a bonding layer, and stacking the bonding layer between two polyvinyl chloride sheets to obtain a stacked composite layer;

[0078] S3. Place the composite layer obtained in S2 into a mold, hot-press at 190° C. for 2 h, gradually cool, and demold to obtain a flexible photovoltaic backsheet.

[0079] In this embodiment, a flexible photovoltaic backplane with a 7-layer structure is finally obtained.

[0080] The flexible photovoltaic backsheet obtained in Examples 1-3 has a simple structure, good bonding, no delamination after testing, and is resistant to boiling water, and no delamination bubbles will be generated after long-term boiling. The flexible photovoltaic backsheet combines the high rigidity of epoxy resin glass fiber composite material and the flexibility of polyvinyl chloride, and has excellent support and protection for the battery sheet.

[0081] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for manufacturing a flexible photovoltaic backsheet, characterized in that: The following steps are involved: S1, obtaining an epoxy resin composition and a glass fiber cloth, uniformly coating the epoxy resin composition on the glass fiber cloth, baking, cooling, obtaining a semi-finished product, and cutting the semi-finished product according to size requirements to obtain an epoxy resin glass fiber prepreg; S2, obtaining a first polyvinyl chloride board and a second polyvinyl chloride board, using the epoxy resin glass fiber prepreg as a bonding layer, and stacking the bonding layer between the first polyvinyl chloride board and the second polyvinyl chloride board to obtain a stacked composite layer; S3, placing the composite layer into a mold, hot pressing, and obtaining a target product; The epoxy resin composition comprises a main epoxy resin, a curing agent, a reaction accelerator, a bonding promoter and a solvent, wherein the main epoxy resin comprises at least one of bisphenol A epoxy resin, bisphenol F epoxy resin, o-cresol epoxy resin, bisphenol A novolac epoxy resin, bromine-containing epoxy resin and phosphorus-containing epoxy resin, and the bonding promoter comprises one or more of thermoplastic acrylate, thermoplastic phenoxy resin, liquid rubber, modified nitrile rubber, nitrile rubber modified epoxy resin, polyurethane modified epoxy resin and polyvinyl acetal.

2. The method for manufacturing a flexible photovoltaic backsheet according to claim 1, characterized in that: The glass fiber cloth is an electronic grade alkali-free glass fiber cloth, and the gram weight of the electronic grade alkali-free glass fiber cloth is 48-220g / m 2 .

3. The method for manufacturing a flexible photovoltaic backsheet according to claim 1, characterized in that: The curing agent includes one or more of dicyandiamide, phenolic resin, 4,4'-diaminodiphenyl sulfone and acid anhydride.

4. The method for manufacturing a flexible photovoltaic backsheet according to claim 1, characterized in that: The reaction accelerator includes one or more of 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, organic urea and 2,4,6-tris(dimethylaminomethyl)phenol.

5. The method for manufacturing a flexible photovoltaic backsheet according to claim 1, characterized in that: The solvent includes one or more of acetone, butanone, ethylene glycol monomethyl ether, propylene glycol methyl ether and N,N-dimethylformamide.

6. The method for manufacturing a flexible photovoltaic backsheet according to claim 1, characterized in that: The resin content of the epoxy resin glass fiber prepreg is 30-70%.

7. The method for manufacturing a flexible photovoltaic backsheet according to claim 1, characterized in that: The epoxy resin composition further comprises functional additives, and the functional additives include one or more of flame retardants, pigments, inorganic fillers, antioxidants, ultraviolet absorbers or light stabilizers.

8. The method for manufacturing a flexible photovoltaic backsheet according to claim 7, characterized in that: The flame retardant includes one or more of tetrabromobisphenol A, organic phosphorus, melamine phosphate, melamine cyanurate, aluminum hydroxide and magnesium hydroxide.

9. The method for manufacturing a flexible photovoltaic backsheet according to claim 1, characterized in that: In S2, a plurality of epoxy resin glass fiber prepreg sheets are stacked in the bonding layer.

10. A flexible photovoltaic backsheet, characterized in that: The flexible photovoltaic backsheet is prepared according to the manufacturing method of any one of claims 1-9.