A hollow carbon fiber composite material for catalyzing nitrate reduction to produce ammonia, and a preparation method and application thereof

By loading copper and nickel nanoclusters on hollow carbon fibers, the problems of high energy consumption and environmental pollution of existing ammonia production methods are solved, and efficient ammonia production and catalytic performance are achieved.

CN118253305BActive Publication Date: 2024-11-12LANZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410403694.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-03
Publication Date
2024-11-12
Estimated Expiration
2044-04-03

AI Technical Summary

Technical Problem

Existing ammonia production methods such as the Haber-Bosch process have high energy consumption and serious environmental pollution, low efficiency of electrocatalytic nitrate reduction reactions, and there are problems such as competitive hydrogen evolution reactions to reduce ammonia selectivity and Faraday efficiency.

Method used

Using a carbon fiber composite with a porous hollow structure, supported copper and nickel nanoclusters as electrocatalysts, it is prepared by electrospinning and two-stage heat treatment, and is used to electrochemically catalyze nitrate reduction to produce ammonia.

Benefits of technology

The catalytic activity and ammonia yield are improved, energy consumption is reduced, and the efficiency of catalyst utilization and energy efficiency are achieved through regulating the proportion of metal clusters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004776428350000011
    Figure HDA0004776428350000011
  • Figure HDA0004776428350000012
    Figure HDA0004776428350000012
  • Figure HDA0004776428350000021
    Figure HDA0004776428350000021
Patent Text Reader

Abstract

The present invention provides a hollow carbon fiber composite material that can be used for nitrate reduction to produce ammonia, and a preparation method and application thereof. The composite material of the present invention comprises a substrate and a metal atom cluster supported on the substrate, wherein the substrate comprises a carbon fiber with a multi-porous hollow structure inside, and the metal comprises copper and / or nickel. The composite material of the present invention exhibits excellent catalytic activity in the nitrate reduction to produce ammonia reaction, and has a high ammonia yield and Faraday efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal catalytic materials, and in particular to a hollow carbon fiber composite material that can be used for catalyzing nitrate reduction to produce ammonia, and a preparation method and application thereof. Background Art

[0002] Ammonia (NH 3 ) is an important chemical product, playing an irreplaceable role in various fields such as industry and agriculture. In addition, due to the 3 The hydrogen content of NH is high (17.6%), the energy density is high (4.3kWh / kg), and it can also be used as an energy storage material and energy carrier. 3 The most common industrial production method is the Haber-Bosch process, which uses N 2 and H 2 As raw materials, iron-based materials are used to catalyze the reaction. However, the Haber-Bosh process relies on high temperature and high pressure reaction conditions (400-500°C, 100-200atm), consumes 1% of the world's annual energy output, releases a large amount of greenhouse gases, and causes harm to the environment.

[0003] In recent years, electrocatalytic and photocatalytic nitrogen reduction to produce NH 3 As a green and environmentally friendly method, it has also been widely studied. However, due to the low water solubility of nitrogen, the extremely high bond energy of N≡N (940.95 kJ / mol) and the high reaction energy barrier, NH 3 The yield is low and the energy efficiency is not satisfactory. At present, another method for producing ammonia is the electrocatalytic nitrate (NO 3 - ) reduction reaction (NO 3 - RR), NO 3 - Due to its high water solubility and low N=O bond energy (204 kJ / mol), NO 3 - RR is more efficient. In addition, due to nitrogen-containing pollutants, especially NO 3 - The increasing emissions of NOx pose a potential threat to the natural environment and human health. 3 - The accumulation of NO in water bodies causes algae to grow in large quantities, the dissolved oxygen content in the water body to decrease, a large number of aquatic plants and animals die, and anaerobic bacteria begin to grow in large quantities, deteriorating water quality. 3 - In the human body, it can be converted into nitrite (NO 2 -), which can oxidize the iron atoms in hemoglobin into trivalent iron, thereby converting hemoglobin into methemoglobin, which has no ability to bind and transport oxygen, causing methemoglobinemia, NO 2 - It may also be converted into strong carcinogenic nitrosamines in the human body. 3 - RR can not only produce valuable NH 3 It can also degrade nitrogen-containing pollutants in the environment and promote the nitrogen cycle in the ecosystem.

[0004] However, NO 3 - The electrochemical equation of RR is NO 3 - +6H 2 O+8e - →NH 3 +9OH - , involving a complex transfer process of eight electron-coupled protons, while the competing hydrogen evolution reaction (HER) reduces NH 3 Therefore, it is necessary to construct reasonable and efficient electrocatalysts to improve NO 3 - Recently, copper-based materials have been widely studied because copper exhibits an inhibitory effect on HER and copper is a NO 3 - Copper is one of the most active metals for RR, and has highly occupied d orbitals that can effectively absorb NO 3 - In addition, various bimetallic electrocatalysts have shown significant performance in NO compared to pure metal electrocatalysts. 3 - RR shows more perfect performance. This is because bimetallic electrocatalysis can effectively adjust the d-band center of the entire structure and improve the adsorption strength between the bimetallic active sites and intermediates through the synergistic effect between atoms. In addition, the substrate also has a great influence on the activity of the catalyst. Currently, a large number of metal substrates have been reported, which can enhance the catalyst. However, the metal substrate consumes more metal resources than the catalyst, which greatly increases its cost and reduces its sustainability. Summary of the invention

[0005] In order to solve one of the above technical problems existing in the prior art, the present invention provides a metal cluster / carbon fiber composite material and its preparation method and application. The composite material of the present invention is based on a carbon fiber with a multi-porous hollow structure, loaded with copper nanoclusters and nickel nanoclusters, and is used for electrochemical catalysis of NO 3 - Reduction to NH 3, with higher catalytic activity and ammonia yield.

[0006] A first aspect of the present invention provides a hollow carbon fiber composite material, which includes a substrate and metal atom clusters supported on the substrate, wherein the substrate includes carbon fibers with a multi-porous hollow structure inside, and the metal includes copper and / or nickel.

[0007] According to some embodiments of the present invention, the metal includes copper and nickel. When the metal includes both copper and nickel, the electrochemical catalysis of NO is more efficient than that of the metal containing only copper or nickel. 3 - Reduction to NH 3 , with higher catalytic activity and ammonia yield.

[0008] According to some embodiments of the present invention, the composite material further comprises copper single atoms and / or nickel single atoms supported on the substrate.

[0009] According to some embodiments of the present invention, in every 100 mg of the composite material, the total mass of metallic copper and / or nickel is 1-4 mg.

[0010] According to some embodiments of the present invention, in the composite material, based on the total mass of copper element and nickel element, the mass proportion of nickel element is 0-100%, for example, 0, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 50%, 60%, 70%, 80%, 90%, 100% or any value therebetween.

[0011] According to some embodiments of the present invention, in the composite material, based on the total mass of copper and nickel, the mass proportion of nickel is 15-35%, for example, 15%, 20%, 25%, 30%, 35%, etc., preferably 20-25%.

[0012] According to some embodiments of the present invention, in the composite material, the mass proportion of copper element, calculated on the total mass of copper element and nickel element, is 0-100%, for example, 0, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 50%, 60%, 70%, 80%, 90%, 100% or any value therebetween.

[0013] According to some embodiments of the present invention, in the composite material, based on the total mass of copper and nickel, the mass proportion of copper is 65-85%, for example, 65%, 70%, 75%, 80%, 85%, etc., preferably 75-80%.

[0014] According to some embodiments of the present invention, the average diameter of the carbon fiber is 100-800 nm. In some embodiments, the average diameter of the carbon fiber is 300-600 nm. In some embodiments, the average diameter of the carbon fiber is 400-600 nm.

[0015] According to some embodiments of the present invention, the average pore size of the pores in the carbon fiber is 10-50 nm, for example, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, etc.

[0016] According to some embodiments of the present invention, the average size of the metal atom clusters is 1-4 nm, preferably 0.5-1.5 nm.

[0017] A second aspect of the present invention provides a method for preparing a hollow carbon fiber composite material, comprising the following steps:

[0018] Electrospinning a spinning solution containing a metal precursor and a first carbon precursor to obtain a spinning sample; wherein the metal precursor includes a copper precursor and / or a nickel precursor, and the first carbon precursor includes one or more of polystyrene, paraffin oil, and polyvinyl acetate;

[0019] The spun sample is dried and subjected to a two-stage heat treatment to obtain the composite material.

[0020] According to some embodiments of the present invention, the metal precursor includes both a copper precursor and a nickel precursor.

[0021] According to some embodiments of the present invention, the copper precursor includes one or both of copper acetylacetonate and copper acetate.

[0022] According to some embodiments of the present invention, the nickel precursor includes one or both of nickel acetylacetonate and nickel acetate.

[0023] According to some embodiments of the present invention, the mass ratio of the copper precursor to the nickel precursor is 1:(0-∞). In the present invention, the loading of metal atom clusters of different proportions on the hollow carbon fiber can be achieved by adjusting the usage ratio of the copper precursor and the nickel precursor. In some preferred embodiments, the mass ratio of the copper precursor to the nickel precursor is 1:(0.5-2), more preferably 1:(0.8-1.2).

[0024] According to some embodiments of the present invention, the spinning solution further includes a second carbon precursor, which includes but is not limited to one or more of the following: polyacrylonitrile, polyvinyl pyrrolidone, polyvinyl alcohol, polyethylene glycol, polyurethane, polyacrylic acid, cellulose acetate, methyl cellulose, carboxymethyl cellulose, polyvinylidene fluoride, polymethyl methacrylate, polyacrylamide, polyethylene oxide, polylactic acid, polyamide, polycaprolactone, polyvinyl butyral, polyaniline, polyimide and polycarbonate, etc. In some embodiments, the second carbon precursor includes one or both of polyacrylonitrile and polyvinyl pyrrolidone. In some specific embodiments, the first carbon precursor includes polystyrene, and the second carbon precursor includes polyacrylonitrile. In some specific embodiments, the first carbon precursor includes polystyrene, and the second carbon precursor includes polyvinyl pyrrolidone. In some embodiments, the mass ratio of the first carbon precursor to the second carbon precursor is 1: (0.5-2), preferably 1: (0.8-1.2), for example 1: 1.

[0025] According to some embodiments of the present invention, the ratio of the total mass of the first carbon precursor and the second carbon precursor to the total mass of the copper precursor and / or the nickel precursor is (10-15):1, for example, 10:1, 11:1, 12:1, 13:1, 14:1, 15:1, etc.

[0026] According to some embodiments of the present invention, the ratio of the mass of the first carbon precursor to the total mass of the copper precursor and / or the nickel precursor is (5-10):1, for example 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, etc., preferably (5-8):1.

[0027] According to some embodiments of the present invention, the spinning solution also includes a solvent. The solvent of the present invention includes, but is not limited to, one or more of the following: carboxylic acids, tetrahydrofuran, ketones, alkanes, nitriles, halogenated alkanes, alcohols, aromatic hydrocarbons, amines, sulfoxides, amides, etc. Examples of the solvent of the present invention include, but are not limited to, formic acid, tetrahydrofuran, acetone, acetylacetone, butanone, n-hexane, cyclohexane, n-heptane, acetonitrile, N-methylpyrrolidone, 1,2-propylene glycol, chloroform, dichloromethane, 1,2-dichloroethane, methanol, ethanol, isopropanol, 1-methoxy-2-propanol, tert-butyl alcohol, n-butyl alcohol, n-propyl alcohol, toluene, xylene, ethylenediamine, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, and carbon tetrachloride, etc. In some preferred embodiments, the solvent includes one or both of N,N-dimethylformamide and N,N-dimethylacetamide.

[0028] According to some embodiments of the present invention, the ratio of the mass of the first carbon precursor to the volume of the solvent is 1:(9-13) g / mL, for example 1:9 g / mL, 1:10 g / mL, 1:11 g / mL, 1:12 g / mL, 1:13 g / mL, etc.

[0029] According to some embodiments of the present invention, the preparation of the spinning solution comprises the following steps:

[0030] S1. mixing the first carbon precursor and the second carbon precursor with the solvent to obtain a mixed solution;

[0031] S2. Mixing the mixed solution with the metal precursor to obtain a spinning solution.

[0032] In some embodiments, the mixing temperature in step S1 is 20-35° C., and the mixing time is 1-4 hours, such as 1 hour, 2 hours, 3 hours, 4 hours, etc.

[0033] In some embodiments, the mixing temperature in step S2 is 20-35° C., and the mixing time is 20-30 hours, such as 20 hours, 22 hours, 24 hours, 26 hours, 28 hours, 30 hours, etc.

[0034] According to some embodiments of the present invention, the electrospinning conditions include: voltage 12-20 kV, flow rate 0.01-0.1 mL·min -1 .

[0035] According to some embodiments of the present invention, the drying temperature is 40-90°C, for example 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, etc.

[0036] According to some embodiments of the present invention, the two-stage heat treatment includes a first stage heat treatment and a second stage heat treatment, wherein the temperature of the first stage heat treatment is 150-250°C, for example, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C, etc., and the temperature of the second stage heat treatment is 850-950°C, for example, 850°C, 860°C, 870°C, 880°C, 890°C, 900°C, 910°C, 920°C, 930°C, 940°C, 950°C, etc.

[0037] In the method of the present invention, the first stage heat treatment is used to stabilize the structure of the prepared nanofibers to avoid fiber breakage during the subsequent high-temperature carbonization process, and the second stage heat treatment is used to carbonize the fibers at high temperature.

[0038] According to some embodiments of the present invention, the temperature of the first stage heat treatment is 180-220°C.

[0039] According to some embodiments of the present invention, the temperature of the second stage heat treatment is 880-920°C.

[0040] According to some embodiments of the present invention, the time of the first stage heat treatment is 2-4 hours.

[0041] According to some embodiments of the present invention, the duration of the second stage heat treatment is 2-4 hours.

[0042] According to some embodiments of the present invention, the first stage of heat treatment is performed in an air atmosphere.

[0043] According to some embodiments of the present invention, the heat treatment in the second stage is carried out in a reducing atmosphere and / or an inert atmosphere. According to some embodiments of the present invention, the reducing atmosphere comprises hydrogen. According to some embodiments of the present invention, the inert atmosphere comprises one or more of nitrogen, argon, and helium. According to some embodiments of the present invention, the heat treatment in the second stage is carried out in a reducing and inert mixed gas, such as a mixed gas of hydrogen and argon.

[0044] The hollow carbon fiber composite material can be obtained by the above method of the present invention, and the composite material includes a carbon fiber substrate with a multi-porous hollow structure inside and copper atom clusters and / or nickel atom clusters supported on the carbon fiber substrate. By selecting a specific first carbon precursor type and controlling the carbonization temperature within a suitable range, the preparation of the carbon fiber substrate with a multi-porous hollow structure inside can be achieved.

[0045] In some embodiments, the hollow carbon fiber composite material further includes copper single atoms and / or nickel single atoms supported on the carbon fiber substrate.

[0046] The third aspect of the present invention provides the use of the hollow carbon fiber composite material described in the first aspect or the hollow carbon fiber composite material prepared by the method described in the second aspect in catalyzing nitrate reduction to produce ammonia.

[0047] Compared with the prior art, the present invention has the following beneficial technical effects:

[0048] 1. The composite material provided by the present invention has a substrate of carbon fiber (lotus root-shaped hollow structure) with a multi-porous hollow structure inside. This unique structure makes the material have a smaller size and a larger specific surface area, which can provide more reactive sites and reactive areas in the catalytic reaction, promote the transmission of electrons, and improve the catalytic performance and catalytic efficiency of the material. In addition, the active components of the composite material are copper and nickel in the form of atomic clusters (monoatom form), which can give full play to the catalytic activity of each atom in the catalytic reaction and improve the atomic utilization rate.

[0049] 2. The preparation method of the composite material of the present invention is simple and easy to operate. The ratio between the loaded metal clusters can be adjusted as needed, and the amount of metal used is extremely low, which greatly improves the utilization rate of atoms and is conducive to mass production and promotion and application.

[0050] 3. The composite material provided by the present invention exhibits excellent electrochemical catalysis of NO 3 - RR performance, can produce NH in large quantities 3 , and has high energy efficiency. The ammonia yield can reach 242.64 μmol h at -0.7 V. -1 mg -1 , the Faraday efficiency can reach 89.29%. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 The scanning electron microscope image and the transmission electron microscope image of the product prepared in Example 1 are shown.

[0052] Figure 2 The high-resolution transmission electron microscopy image and HAADF-STEM image of the product prepared in Example 1 are shown.

[0053] Figure 3 The morphological characterization results of the products prepared in Example 2 and Example 3 are shown; wherein, Figure (a) and Figure (b) are scanning electron microscope images of the products prepared in Example 2 and Example 3, respectively; Figure (c) and Figure (d) are transmission electron microscope images of the products prepared in Example 2 and Example 3, respectively.

[0054] Figure 4 The XRD patterns of the products prepared in Examples 1 to 3 are shown.

[0055] Figure 5 A high-angle annular dark-field scanning transmission electron microscope image of the product prepared in Example 1 and a corresponding element distribution map are shown.

[0056] Figure 6The spherical aberration-corrected high-angle annular dark-field scanning transmission electron microscope image of the product prepared in Example 1 and the corresponding Cu and Ni element distribution map are shown.

[0057] Figure 7 The electrochemical catalysis of the product prepared in Example 1 to NO 3 - Test results for reduction of ammonia production.

[0058] Figure 8 Comparative results of ammonia yield and Faradaic efficiency of the products prepared in Examples 1 to 3 are shown. DETAILED DESCRIPTION

[0059] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments and drawings. The specific embodiments described herein are only used to explain the present invention and are not intended to constitute any limitation to the present invention.

[0060] The reagents used in the examples and comparative examples, unless otherwise specified, are conventional commercial products or reagents prepared by conventional methods, and the methods used in the examples and comparative examples, unless otherwise specified, are conventional experimental methods. The instruments used in the examples and comparative examples, unless otherwise specified, can all be obtained through commercial channels.

[0061] The term "cluster" used in this article refers to a relatively stable microscopic or submicroscopic aggregate composed of several or even thousands of atoms, molecules or ions through physical or chemical binding forces, and its physical and chemical properties vary with the number of atoms contained. Cluster is a concept of nanomaterials at the material scale. Clusters can be seen as a new level of material structure between atoms, molecules and macroscopic solid substances, and are the transitional state of various substances from atoms and molecules to bulk substances.

[0062] Example 1

[0063] Weigh 630 mg of polystyrene and 630 mg of polyacrylonitrile respectively, dissolve in 7 mL of N,N-dimethylformamide, and stir for 2 hours until the mixture is uniform. Add 50 mg of copper acetylacetonate and 50 mg of nickel acetylacetonate to the mixed solution, stir overnight, and prepare a spinning solution.

[0064] The mixed spinning solution was poured into a disposable syringe and then installed on the electrospinning machine. The distance between the syringe needle and the collector was 15 cm. The high-voltage power supply used a voltage of 14 kV and a flow rate of 0.01 mL min -1 The spun samples were dried in an oven at 60°C.

[0065] The dried spinning sample was pretreated under the experimental conditions of 200°C in air atmosphere for 3 hours, carbonized in a tube furnace after pretreatment, and calcined at 900°C for 3 hours, with hydrogen and argon mixed gas passing into the tube furnace for protection. The product obtained after cooling was a mixed cluster of copper and nickel anchored on the substrate carbon nanotubes. ICP-OES showed that the mass percentages of Ni and Cu were 22.49wt% and 77.51wt%, respectively.

[0066] Example 2

[0067] The difference from Example 1 is that the input of metal salt is different, that is, only 100 mg of copper acetylacetonate is added, and no nickel acetylacetonate is added.

[0068] Example 3

[0069] The difference from Example 1 is that the input of metal salt is different, that is, only 100 mg of nickel acetylacetonate is added, and copper acetylacetonate is not added.

[0070] Comparative Example 1

[0071] The difference from Example 1 is that the spinning sample is directly carbonized without pretreatment after drying. The details are as follows:

[0072] Weigh 630 mg of polystyrene and 630 mg of polyacrylonitrile respectively, dissolve in 7 mL of N,N-dimethylformamide, and stir for 2 hours until the mixture is uniform. Add 50 mg of copper acetylacetonate and 50 mg of nickel acetylacetonate to the mixed solution, stir overnight, and prepare a spinning solution.

[0073] The mixed spinning solution was poured into a disposable syringe and then installed on the electrospinning machine. The distance between the syringe needle and the collector was 15 cm. The high-voltage power supply used a voltage of 14 kV and a flow rate of 0.01 mL min -1 The spun samples were dried in an oven at 60°C.

[0074] The dried spinning sample was placed in a tube furnace for carbonization and calcined at 900°C for 3 hours, with hydrogen and argon mixed gas passing through the tube furnace for protection. After cooling, the fiber structure of the product was partially destroyed.

[0075] 1. Characterization of product morphology, structure and composition

[0076] The scanning electron microscope image and transmission electron microscope image of the product obtained in Example 1 are as follows: Figure 1 and Figure 2 shown.

[0077] from Figure 1From the scanning electron microscope cross-sectional image of a, we can see that the product is a hollow and porous lotus root-like structure, and the diameter of the nanotube is about 500nm, indicating that the metal doping does not affect the morphology and structure of the carbon nanotube. Figure 1 b The porous hollow structure of the nanotubes can be seen more clearly in the transmission electron microscope image, and the pore diameter is about 30nm.

[0078] from Figure 2 Lattice fringes cannot be observed in the high-resolution transmission electron microscope image of a, indicating that it is an amorphous carbon material. Through the high-angle annular dark field scanning transmission mode of the spherical aberration electron microscope, multiple bright spots can be observed together, as well as a single bright spot (red circle), indicating that copper and nickel elements exist on the surface of carbon nanotubes in the form of atomic clusters and single atoms.

[0079] The scanning electron microscope image and transmission electron microscope image of the product prepared in Example 2 are as follows: Figure 3 (a) and Figure 3 The scanning electron microscope image and transmission electron microscope image of the product prepared in Example 3 are shown in Figure 3 (b) and Figure 3 (d) As shown in the SEM image, the samples are all hollow and porous lotus root-like structures, and the diameter of the nanotubes is about 500nm, indicating that the doping of copper and nickel metals has not affected the morphology and structure of carbon nanotubes. No aggregation of nanoparticles was observed from the TEM image, and the porous hollow structure of the nanotubes can be seen more clearly, and the pore diameter is about 30nm.

[0080] The XRD spectra of the product prepared in Example 1, the product prepared in Example 2 and the product prepared in Example 3 do not have additional diffraction peaks (see Figure 4 ), indicating that no copper or nickel nanoparticles are generated, and the materials exist in an amorphous form. The peak at 2θ=25° in the figure corresponds to the (002) crystal plane of carbon, indicating its amorphous carbon structure, which corresponds to the high-resolution transmission electron microscope image. However, for the doped copper and nickel metals, there is no diffraction peak at the corresponding position of the standard PDF card, indicating that no copper or nickel nanoparticles are generated, but smaller metal clusters are formed, which further verifies the conclusion of the HAADF-STEM image.

[0081] High-angle annular dark field scanning transmission electron microscope image and element distribution map of the product prepared in Example 1 ( Figure 5 ) shows that copper and nickel are evenly distributed, proving the successful incorporation of copper and nickel. From the spherical aberration corrected high-angle annular dark field scanning transmission electron microscopy image and element distribution ( Figure 6 ) found that copper and nickel elements are clustered together, not completely dispersed, which is consistent with Figure 2b is consistent with the HADDF-STEM image, proving that some copper and nickel exist on the carbon nanotubes in the form of small clusters.

[0082] 2. Electrochemical Catalysis of NO 3 - RR property test

[0083] The three products prepared in Examples 1 to 3 were used as catalysts for electrochemical catalysis of NO 3 - RR property test, the test method is as follows:

[0084] Use 0.1M KNO 3 The catalyst prepared in Example 1-3 was loaded on carbon paper (1 mg / sheet) as the working electrode, a platinum sheet electrode was used as the counter electrode, and a mercury / mercuric oxide electrode was used as the reference electrode to carry out an electrocatalytic reaction in an H-type electrolytic cell. The electrocatalytic reaction time was 0.5 hours. After the reaction was completed, an appropriate amount of electrolyte was taken to analyze the product concentration in the electrolyte. The results are shown in Figure 7 and Figure 8 shown.

[0085] Figure 7 (a) The results show that the NH 3 The Faradaic efficiency was maintained above 70%, reaching 89.29% at -0.7 V, indicating that the metal cluster-anchored hollow tubular CNT composites have a wide voltage range for NO 3 - Degradation to produce ammonia has good energy efficiency.

[0086] Figure 7 (b) shows the voltage range of NH from -0.4 V to -0.8 V. 3 The yield of NH 3 The yield increased as the applied potential shifted from -0.4 V to a negative value, reaching a maximum of 242.64 μmol h at -0.7 V. -1 mg -1 , and then slightly decreased with the continued increase of the applied potential. This may be because the more negative applied potential promoted the competitive hydrogen evolution reaction, which made NH 3 The highest ammonia yield achieved at -0.7 V is better than most reported materials.

[0087] from Figure 8The results show that compared with Example 3, the products prepared in Example 1 and Example 2 have higher ammonia yield and Faraday efficiency, especially the bimetallic (copper and nickel) loaded catalyst prepared in Example 1 is more effective than the single metal copper loaded catalyst.

[0088] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.

Claims

1. A hollow carbon fiber composite material that can be used to catalyze nitrate reduction to produce ammonia, comprising a substrate and a metal atom cluster supported on the substrate, wherein the substrate comprises a carbon fiber with a multi-porous hollow structure, and the metal comprises copper and nickel; The preparation method of the hollow carbon fiber composite material comprises the following steps: Electrospinning a spinning solution containing a metal precursor, a first carbon precursor and a second carbon precursor to obtain a spinning sample; Drying and two-stage heat treatment of the spinning sample to obtain the composite material; in, The metal precursor includes a copper precursor and a nickel precursor, the copper precursor includes one or both of copper acetylacetonate and copper acetate, and the nickel precursor includes one or both of nickel acetylacetonate and nickel acetate; the mass ratio of the copper precursor to the nickel precursor is 1:(0.5-2); The first carbon precursor includes one or more of polystyrene, paraffin oil, and polyvinyl acetate; the second carbon precursor includes one or two of polyacrylonitrile and polyvinyl pyrrolidone; the mass ratio of the first carbon precursor to the second carbon precursor is 1:(0.5-2); The two-stage heat treatment includes a first stage heat treatment and a second stage heat treatment, wherein the temperature of the first stage heat treatment is 150-250°C, and the temperature of the second stage heat treatment is 850-950°C.

2. The hollow carbon fiber composite material according to claim 1, characterized in that: The composite material further comprises copper single atoms and / or nickel single atoms supported on the substrate; and / or, In every 100 mg of the composite material, the total mass of metal copper and nickel is 1-4 mg.

3. The hollow carbon fiber composite material according to claim 1 or 2, characterized in that: In the composite material, based on the total mass of copper and nickel, the mass of nickel accounts for 15-35% and the mass of copper accounts for 65-85%.

4. The hollow carbon fiber composite material according to claim 1 or 2, characterized in that: In the composite material, based on the total mass of copper and nickel, the mass of nickel accounts for 20-25% and the mass of copper accounts for 75-80%.

5. The hollow carbon fiber composite material according to claim 1 or 2, characterized in that: The average diameter of the carbon fiber is 100-800 nm; and / or, the average pore size of the carbon fiber is 10-50 nm; and / or, the average size of the metal atom cluster is 1-4 nm.

6. The hollow carbon fiber composite material according to claim 5, characterized in that: The average size of the metal atom clusters is 0.5-1.5 nm.

7. The hollow carbon fiber composite material according to claim 1, characterized in that: The mass ratio of the copper precursor to the nickel precursor is 1:(0.8-1.2).

8. The hollow carbon fiber composite material according to claim 1, characterized in that: The spinning solution also includes a solvent; The solvent includes one or more of carboxylic acid, tetrahydrofuran, ketones, alkanes, nitriles, halogenated alkanes, alcohols, aromatic hydrocarbons, amines, sulfoxides, and amides.

9. The hollow carbon fiber composite material according to claim 8, characterized in that: The solvent includes one or more of formic acid, tetrahydrofuran, acetone, acetylacetone, butanone, n-hexane, cyclohexane, n-heptane, acetonitrile, N-methylpyrrolidone, 1,2-propylene glycol, chloroform, dichloromethane, 1,2-dichloroethane, methanol, ethanol, isopropanol, 1-methoxy-2-propanol, tert-butanol, n-butanol, n-propanol, toluene, xylene, ethylenediamine, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide and carbon tetrachloride.

10. The hollow carbon fiber composite material according to claim 9, characterized in that: The solvent includes one or both of N,N-dimethylformamide and N,N-dimethylacetamide.

11. The hollow carbon fiber composite material according to claim 1, characterized in that: The mass ratio of the first carbon precursor to the second carbon precursor is 1:(0.8-1.2).

12. The hollow carbon fiber composite material according to claim 1, characterized in that: The ratio of the mass of the first carbon precursor to the total mass of the copper precursor and / or the nickel precursor is (5-10):

1.

13. The hollow carbon fiber composite material according to claim 12, characterized in that: The ratio of the mass of the first carbon precursor to the total mass of the copper precursor and / or the nickel precursor is (5-8):

1.

14. The hollow carbon fiber composite material according to any one of claims 8 to 10, characterized in that: The ratio of the mass of the first carbon precursor to the volume of the solvent is 1: (9-13) g / mL.

15. The hollow carbon fiber composite material according to claim 8, characterized in that: The preparation of the spinning solution comprises the following steps: S1. mixing the first carbon precursor and the second carbon precursor with the solvent to obtain a mixed solution; S2. Mixing the mixed solution with the metal precursor to obtain a spinning solution.

16. The hollow carbon fiber composite material according to claim 15, characterized in that: The mixing temperature in step S1 is 20-35° C., and the mixing time is 1-4 hours.

17. The hollow carbon fiber composite material according to claim 15, characterized in that: The mixing temperature in step S2 is 20-35° C., and the mixing time is 20-30 hours.

18. The hollow carbon fiber composite material according to claim 1, characterized in that: The electrospinning conditions include: voltage 12-20 kV, flow rate 0.01-0.1 mL·min -1 ; and / or, the drying temperature is 40-90°C; and / or, The two-stage heat treatment includes a first stage heat treatment and a second stage heat treatment, wherein the temperature of the first stage heat treatment is 180-220°C, and the temperature of the second stage heat treatment is 880-920°C; and / or, the time of the first stage heat treatment is 2-4 hours, and the time of the second stage heat treatment is 2-4 hours.

19. The hollow carbon fiber composite material according to claim 18, characterized in that: The first stage heat treatment is carried out in an air atmosphere, and the second stage heat treatment is carried out in a reducing atmosphere and / or an inert atmosphere, wherein the reducing atmosphere includes hydrogen, and the inert atmosphere includes one or more of nitrogen, argon, and helium.