Silicon-free artificial stone and preparation method thereof
Through the combination of unsaturated polyester resin, modified aluminum powder and bamboo fiber, and using surface in-situ coating and activation treatment, the problem of insufficient hardness and aging resistance of silicon-free artificial stone is solved, and high hardness and aging resistance are prepared. Silicon-free artificial stone, suitable for construction and decoration materials.
Patent Information
- Application Number
- CN202410339749.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-03-25
AI Technical Summary
Existing silicon-free artificial stones have defects in hardness, heat resistance and moisture resistance, resulting in the prepared artificial quartz stone having low hardness, easy deformation, and aging, which affects the surface effect and decorative appearance.
Using unsaturated polyester resin, modified aluminum powder and bamboo fiber as the main ingredients, the modified aluminum powder is prepared through in-situ surface coating, activation and modification treatment, combined with vibration degassing and temperature-raising curing processes to prepare high hardness , aging-resistant silicon-free artificial stone.
It improves the hardness, deformation resistance and aging resistance of silicon-free artificial stone, and meets the application needs of polymer synthetic materials in construction and decoration.
Smart Images

Figure BDA0004756336910000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of artificial stone, and in particular to a silicon-free artificial stone and a preparation method thereof. Background Art
[0002] Existing artificial stone slabs can be divided into two categories: artificial quartz slabs and artificial granite (calcium carbonate + resin). Among them, although artificial granite is cheap, its chemical resistance is poor, so its application range is relatively narrow. Artificial quartz stone has excellent mechanical properties and chemical resistance, and has incomparable advantages over artificial granite in terms of moisture resistance and acid resistance. Artificial quartz stone is based on unsaturated polyester resin or thermoplastic polymer, and silicate (type) natural quartz stone and / or powder, silica sand, tailings and other inorganic materials (whose main component is silicon dioxide) are used as the main filler. It is an artificial stone with certain specifications, sizes and shapes processed by a specific process. It is a new type of building and decorative material that is non-radioactive, reusable, environmentally friendly, and green.
[0003] Traditional artificial stone is generally made of quartz, resin, coupling agent, curing agent, etc. Silicon-free artificial stone is a polymer synthetic material composed of aluminum powder, resin and other additives. Unlike traditional artificial stone, it does not contain silicon components and is made through high temperature and high pressure processes. Therefore, silicon-free artificial stone has unique advantages in some specific application scenarios and is widely used in kitchen countertops, bathroom decorations, interior walls and commercial spaces. Silicon-free artificial stone is a polymer synthetic material composed of aluminum powder, resin and other additives, but unlike traditional artificial stone, it does not contain silicon components. Therefore, silicon-free artificial stone has unique advantages in some specific application scenarios.
[0004] At present, silicon-free artificial stone is usually composed of aluminum powder, resin and other additives. The resin is usually unsaturated polyester, which has high mechanical strength and is easy to process, but has defects such as large shrinkage, poor heat resistance and poor moisture resistance. In addition, the aluminum powder has insufficient dispersibility and easy reaction, resulting in the prepared artificial quartz stone having low hardness, easy deformation, easy aging and other problems, which seriously affects the surface effect of the artificial quartz stone and affects the appearance of buildings and interior decoration. Summary of the invention
[0005] In view of the problems existing in the prior art, the object of the present invention is to provide a silicon-free artificial stone and a preparation method thereof.
[0006] The purpose of the present invention is achieved by adopting the following technical solutions:
[0007] In a first aspect, the present invention discloses a silicon-free artificial stone, which comprises the following components calculated by weight:
[0008] 28-36 parts of unsaturated polyester resin, 56-72 parts of reinforcing filler, 3-8 parts of bamboo fiber, 1.6-4 parts of curing agent and 0.5-3.5 parts of pigment.
[0009] Preferably, the unsaturated polyester resin is any one or more combinations of orthophthalic unsaturated polyester resin, isophthalic unsaturated polyester resin, xylene unsaturated polyester resin, and bisphenol A unsaturated polyester resin.
[0010] More preferably, the brand of the orthophthalic unsaturated polyester resin is unsaturated resin 199 or unsaturated resin 196; the brand of the isophthalic unsaturated polyester resin is unsaturated resin 199; the brand of the xylene unsaturated polyester resin is unsaturated polyester resin Xm-1 or unsaturated polyester resin Xm-2; and the brand of the bisphenol A unsaturated polyester resin is unsaturated polyester resin 197.
[0011] Preferably, the reinforcing filler is modified aluminum powder, which is prepared with aluminum powder as the base material, wherein the aluminum content of the aluminum powder is greater than 99% and the particle size is 60-80 μm.
[0012] Preferably, the density of the bamboo fiber is 0.78 g / cm 3 , whiteness is 60.1%, length is 5-10mm, and diameter is 20-30μm.
[0013] Preferably, the curing agent is any one of 2-methyl ethyl peroxide, dibenzoyl peroxide, and tert-butyl perbenzoate.
[0014] Preferably, the pigment is an organic pigment, including one or more combinations of Pigment Yellow 139, Pigment Red 179, Pigment Blue 15, and Pigment Green 7.
[0015] Preferably, the preparation method of the reinforcing filler comprises:
[0016] S1. Surface in-situ coating:
[0017] At room temperature, magnesium acetate is dissolved in anhydrous ethanol to obtain a mixed solution A; aluminum powder is dispersed in an ionic liquid [Bmim] BF4 to obtain a mixed solution B; under the protection of argon, the mixed solution B is added to the mixed solution A, and after being fully stirred, sodium borohydride is added, and the mixture is stirred and dispersed at room temperature for 10-20 hours. After the reaction is completed, the reaction solution is filtered to collect the solid, and after washing and drying, a MgB / Al composite powder is obtained;
[0018] S2. Activation treatment:
[0019] The MgB / Al composite powder is mixed in anhydrous ethanol, heated to reflux for 1-2 hours, the reaction liquid is filtered to collect the solid, and dried under reduced pressure to obtain active MgB / Al;
[0020] Mix active MgB / Al, amino coupling agent and deionized water in a flask, heat to 40-60°C and stir for 3-6 hours, filter the reaction solution to collect the solid, wash and dry to obtain the amino MgB / Al composite powder;
[0021] S3, modification treatment:
[0022] Dissolve bisphenol A diglycidyl ether in N,N-dimethylformamide, add amino MgB / Al composite powder, disperse evenly, heat to 60-80°C, stir for 6-12h, after the reaction is completed, filter the reaction solution to collect the solid, wash and dry to obtain modified aluminum powder, i.e., reinforced filler.
[0023] Preferably, in S1, the ionic liquid [Bmim]BF4 is 1-butyl-3-methylimidazolium tetrafluoroborate, and the mass volume ratio of aluminum powder, magnesium acetate, anhydrous ethanol and ionic liquid [Bmim]BF4 is 1g:(0.14-0.28)g:(5-10)mL:(10-20)mL.
[0024] Preferably, in S1, sodium borohydride is added in multiple times within half an hour, and the added amount is 10%-20% of the mass of magnesium acetate.
[0025] Preferably, in the preparation process of the active MgB / Al in S2, the mass volume ratio of the MgB / Al composite powder and anhydrous ethanol is 1 g:(10-20) mL.
[0026] Preferably, in the preparation process of the amino MgB / Al composite powder in S2, the amino coupling agent is KH-550, and the mass volume ratio of active MgB / Al, amino coupling agent and deionized water is 1g:(0.2-0.3)g:(10-20)mL.
[0027] Preferably, in S3, the mass ratio of the amidated MgB / Al composite powder, bisphenol A diglycidyl ether and N,N-dimethylformamide is 1 g: (0.34-0.48) g: (10-20) mL.
[0028] In a second aspect, the present invention discloses a method for preparing silicon-free artificial stone, comprising the following steps:
[0029] (1) firstly mixing reinforcing filler, bamboo fiber and unsaturated polyester resin in a stirrer, stirring evenly, then adding pigment and curing agent, stirring evenly again, to obtain a premix;
[0030] (2) The premix is introduced into a mold, vibrated and degassed, pressed into shape, and then heated and cured to obtain a silicon-free artificial stone material.
[0031] Preferably, the curing temperature is 60-80° C. and the curing time is 1-3 hours.
[0032] The beneficial effects of the present invention are:
[0033] 1. The present invention prepares a silicon-free artificial stone material, which adopts unsaturated polyester as the resin material, the main reinforcing filler is modified aluminum powder, and the auxiliary reinforcing filler is bamboo fiber. The preparation process does not use natural components in natural stone or quartz stone, which can reduce dependence on natural resources. The prepared artificial stone material has high hardness, is not easy to deform, and has excellent aging resistance.
[0034] 2. The performance of traditional silicon-free artificial stone often cannot meet the requirements due to the resin and aluminum powder in it. This application modifies the main filler aluminum powder, including in-situ coating and surface activation modification. Among them, in-situ coating is to use organic magnesium salt and boron-containing ionic liquid to react on the surface of aluminum powder particles, so as to generate magnesium boride in situ; surface activation modification is to first amino the surface of the coated aluminum powder, and then use bisphenol A diglycidyl ether containing epoxy group to cross-link the reaction, and finally obtain modified aluminum powder.
[0035] 3. In the in-situ coating process of aluminum powder, magnesium acetate is used as the magnesium source and the ionic liquid [Bmim] BF4 is used as the boron-containing reaction medium. Under the action of sodium borohydride at room temperature, a magnesium boride layer is in-situ generated on the surface of the aluminum powder particles to obtain MgB-Al composite powder.
[0036] 4. During the surface activation treatment of MgB-Al powder, the MgB-Al powder is first refluxed with ethanol, one purpose of which is to remove the ionic liquid residue in the MgB-Al powder, and the other purpose is to activate the MgB-Al powder and greatly enhance the surface activity of the MgB-Al powder; then, the MgB-Al powder is treated with an aminosilane coupling agent to obtain an amination MgB-Al powder. DETAILED DESCRIPTION
[0037] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0038] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0039] Some of the materials used in the examples include:
[0040] The aluminum content of the aluminum powder used is >99%, and the particle size is 60-80μm; the density of bamboo fiber is 0.78g / cm 3 , whiteness is 60.1%, length is 5-10mm, and diameter is 20-30μm.
[0041] The unsaturated polyester resin 199 has a solid content of 66±3%, a viscosity of 0.3-0.4 Pa·s / 25°C, and an acid value of 22±2 mgKOH / g.
[0042] The present invention will be further described below in conjunction with the following examples.
[0043] Example 1
[0044] A silicon-free artificial stone, calculated by weight, comprises the following components:
[0045] 32 parts of unsaturated polyester resin 199, 65 parts of reinforcing filler, 5 parts of bamboo fiber, 2.9 parts of curing agent (2-methyl peroxide), 1.2 parts of pigment yellow 139 and 0.8 parts of pigment red 179.
[0046] Wherein, the preparation method of the reinforcing filler comprises:
[0047] S1. Surface in-situ coating:
[0048] At room temperature, magnesium acetate is dissolved in anhydrous ethanol to obtain a mixed solution A; aluminum powder is dispersed in an ionic liquid [Bmim] BF4 (1-butyl-3-methylimidazolium tetrafluoroborate, purity 97.0% (HPLC)), the mass volume ratio of aluminum powder, magnesium acetate, anhydrous ethanol and ionic liquid [Bmim] BF4 is 1g:0.21g:10mL:20mL, to obtain a mixed solution B; under the protection of argon, the mixed solution B is added to the mixed solution A, after fully stirring, sodium borohydride is added several times within half an hour, the added amount is 15% of the mass of magnesium acetate, and the mixture is stirred and dispersed at room temperature for 15h. After the reaction is completed, the reaction solution is filtered to collect the solid, and after washing and drying, MgB / Al composite powder is obtained;
[0049] S2. Activation treatment:
[0050] The MgB / Al composite powder was mixed in anhydrous ethanol, the mass volume ratio of the MgB / Al composite powder to the anhydrous ethanol was 1 g:15 mL, the temperature was raised to reflux for 1.5 h, the reaction solution was filtered to collect the solid, and the solid was dried under reduced pressure to obtain active MgB / Al;
[0051] Active MgB / Al, KH-550 and deionized water were mixed in a flask, the mass volume ratio of active MgB / Al, KH-550 and deionized water was 1g:0.2g:10mL, the temperature was raised to 50°C and stirred for 4h, the reaction solution was filtered to collect the solid, and after washing and drying, the aminated MgB / Al composite powder was obtained;
[0052] S3, modification treatment:
[0053] Dissolve bisphenol A diglycidyl ether in N,N-dimethylformamide, add amide MgB / Al composite powder, the mass ratio of amide MgB / Al composite powder, bisphenol A diglycidyl ether and N,N-dimethylformamide is 1g:0.41g:15mL, after uniform dispersion, heat to 70°C, stir for 8h, after the reaction is completed, filter the reaction solution to collect the solid, wash and dry to obtain modified aluminum powder, i.e., reinforced filler.
[0054] The method for preparing the silicon-free artificial stone comprises the following steps:
[0055] (1) firstly mixing reinforcing filler, bamboo fiber and unsaturated polyester resin in a stirrer, stirring evenly, then adding two pigments and a curing agent, stirring evenly again, to obtain a premix;
[0056] (2) The premix is introduced into a mold, vibrated and degassed, pressed into shape, and then heated to 70° C. for curing for 2 h to obtain a silicon-free artificial stone material.
[0057] Example 2
[0058] A silicon-free artificial stone, calculated by weight, comprises the following components:
[0059] 28 parts of unsaturated polyester resin 196, 56 parts of reinforcing filler, 3 parts of bamboo fiber, 1.6 parts of curing agent (dibenzoyl peroxide), 0.3 parts of pigment red 179 and 0.6 parts of pigment green 7.
[0060] Wherein, the preparation method of the reinforcing filler comprises:
[0061] S1. Surface in-situ coating:
[0062] At room temperature, magnesium acetate is dissolved in anhydrous ethanol to obtain a mixed solution A; aluminum powder is dispersed in an ionic liquid [Bmim]BF4 (1-butyl-3-methylimidazolium tetrafluoroborate, purity 97.0% (HPLC)), the mass volume ratio of aluminum powder, magnesium acetate, anhydrous ethanol and ionic liquid [Bmim]BF4 is 1g:0.14g:5mL:10mL, to obtain a mixed solution B; under the protection of argon, the mixed solution B is added to the mixed solution A, after fully stirring, sodium borohydride is added several times within half an hour, the added amount is 10% of the mass of magnesium acetate, and the mixture is stirred and dispersed at room temperature for 10-20h. After the reaction is completed, the reaction solution is filtered to collect the solid, and after washing and drying, MgB / Al composite powder is obtained;
[0063] S2. Activation treatment:
[0064] The MgB / Al composite powder is mixed in anhydrous ethanol, the mass volume ratio of the MgB / Al composite powder to the anhydrous ethanol is 1g:10mL, the temperature is raised to reflux for 1h, the reaction liquid is filtered to collect the solid, and the solid is dried under reduced pressure to obtain active MgB / Al;
[0065] Active MgB / Al, KH-550 and deionized water were mixed in a flask, the mass volume ratio of active MgB / Al, KH-550 and deionized water was 1g:0.2g:10mL, the temperature was raised to 40°C and stirred for 3h, the reaction solution was filtered to collect the solid, and after washing and drying, the aminated MgB / Al composite powder was obtained;
[0066] S3, modification treatment:
[0067] Dissolve bisphenol A diglycidyl ether in N,N-dimethylformamide, add amide MgB / Al composite powder, the mass ratio of amide MgB / Al composite powder, bisphenol A diglycidyl ether and N,N-dimethylformamide is 1g:0.34g:10mL, after uniform dispersion, heat to 60°C, stir for 6h, after the reaction is completed, filter the reaction solution to collect the solid, wash and dry to obtain modified aluminum powder, i.e., reinforced filler.
[0068] The method for preparing the silicon-free artificial stone comprises the following steps:
[0069] (1) firstly mixing reinforcing filler, bamboo fiber and unsaturated polyester resin in a stirrer, stirring evenly, then adding pigment and curing agent, stirring evenly again, to obtain a premix;
[0070] (2) The premix is introduced into a mold, vibrated and degassed, pressed into shape, and then heated to 60° C. for curing for 3 h to obtain a silicon-free artificial stone material.
[0071] Example 3
[0072] A silicon-free artificial stone, calculated by weight, comprises the following components:
[0073] 36 parts of unsaturated polyester resin 197, 72 parts of reinforcing filler, 8 parts of bamboo fiber, 4 parts of curing agent (tert-butyl perbenzoate) and 3.5 parts of pigment blue.
[0074] Wherein, the preparation method of the reinforcing filler comprises:
[0075] S1. Surface in-situ coating:
[0076] At room temperature, magnesium acetate is dissolved in anhydrous ethanol to obtain a mixed solution A; aluminum powder is dispersed in an ionic liquid [Bmim] BF4 (1-butyl-3-methylimidazolium tetrafluoroborate, purity 97.0% (HPLC)), the mass volume ratio of aluminum powder, magnesium acetate, anhydrous ethanol and ionic liquid [Bmim] BF4 is 1g:0.28g:10mL:20mL, to obtain a mixed solution B; under the protection of argon, the mixed solution B is added to the mixed solution A, after being fully stirred, sodium borohydride is added several times within half an hour, the added amount is 20% of the mass of magnesium acetate, and the mixture is stirred and dispersed at room temperature for 20 hours. After the reaction is completed, the reaction solution is filtered to collect the solid, and after washing and drying, MgB / Al composite powder is obtained;
[0077] S2. Activation treatment:
[0078] The MgB / Al composite powder is mixed in anhydrous ethanol, the mass volume ratio of the MgB / Al composite powder to the anhydrous ethanol is 1g:20mL, the temperature is raised to reflux for 2h, the reaction liquid is filtered to collect the solid, and the solid is dried under reduced pressure to obtain active MgB / Al;
[0079] Active MgB / Al, KH-550 and deionized water were mixed in a flask, the mass volume ratio of active MgB / Al, KH-550 and deionized water was 1g:0.3g:20mL, the temperature was raised to 60°C and stirred for 6h, the reaction solution was filtered to collect the solid, and after washing and drying, the aminated MgB / Al composite powder was obtained;
[0080] S3, modification treatment:
[0081] Dissolve bisphenol A diglycidyl ether in N,N-dimethylformamide, add amide MgB / Al composite powder, the mass ratio of amide MgB / Al composite powder, bisphenol A diglycidyl ether and N,N-dimethylformamide is 1g:0.48g:20mL, after uniform dispersion, heat to 80°C, stir for 12h, after the reaction is completed, filter the reaction liquid to collect the solid, wash and dry to obtain modified aluminum powder, i.e., reinforced filler.
[0082] The method for preparing the silicon-free artificial stone comprises the following steps:
[0083] (1) firstly mixing reinforcing filler, bamboo fiber and unsaturated polyester resin in a stirrer, stirring evenly, then adding pigment and curing agent, stirring evenly again, to obtain a premix;
[0084] (2) The premix is introduced into a mold, vibrated and degassed, pressed into shape, and then heated to 80° C. for curing for 1 hour to obtain a silicon-free artificial stone material.
[0085] Comparative Example 1
[0086] A silicon-free artificial stone, which is different from Example 1 only in that the reinforcing filler is replaced by conventional aluminum powder.
[0087] Comparative Example 2
[0088] A silicon-free artificial stone, which is different from Example 1 only in that the reinforcing filler is replaced by MgB / Al composite powder, and the preparation of the MgB / Al composite powder is the same as step S1 of the example.
[0089] Comparative Example 3
[0090] A silicon-free artificial stone, which differs from Example 1 only in that the reinforcing filler is replaced by a mixture of MgB / Al composite powder and bisphenol A diglycidyl ether, the preparation of the MgB / Al composite powder is the same as step S1 of the example, and the mass ratio of the MgB / Al composite powder to bisphenol A diglycidyl ether is 1:0.41.
[0091] In order to more clearly illustrate the content of the present invention, the performance of the silicon-free artificial stone prepared in Example 1 and Comparative Examples 1-3 was tested. The tensile performance test referred to GB / T2567-2008, and the aging condition was 120°C oven treatment for 3 days. The test results are shown in Table 1.
[0092] Table 1 Performance test results of different silicon-free artificial stones
[0093]
[0094] It can be seen from Table 1 that the hardness, heat deformation resistance, tensile strength and aging resistance of the silicon-free artificial stone prepared in Example 1 of the present invention are better than those of other artificial stones, indicating that the artificial stone manufactured by the present invention has more excellent performance.
[0095] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0096] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A silicon-free artificial stone, characterized in that: Calculated by weight, it includes the following ingredients: 28-36 parts of unsaturated polyester resin, 56-72 parts of reinforcing filler, 3-8 parts of bamboo fiber, 1.6-4 parts of curing agent and 0.5-3.5 parts of pigment; The reinforcing filler is modified aluminum powder, which is prepared by using aluminum powder as the base material and undergoing surface in-situ coating, activation treatment and modification treatment; The preparation method of the reinforcing filler comprises: S1. Surface in-situ coating: At room temperature, magnesium acetate is dissolved in anhydrous ethanol to obtain a mixed solution A; aluminum powder is dispersed in an ionic liquid [Bmim] BF4 to obtain a mixed solution B; under the protection of argon, the mixed solution B is added to the mixed solution A, and after being fully stirred, sodium borohydride is added, and the mixture is stirred and dispersed at room temperature for 10-20 hours. After the reaction is completed, the reaction solution is filtered to collect the solid, and after washing and drying, a MgB / Al composite powder is obtained; S2. Activation treatment: The MgB / Al composite powder is mixed in anhydrous ethanol, heated to reflux for 1-2 hours, the reaction liquid is filtered to collect the solid, and the solid is dried under reduced pressure to obtain active MgB / Al; the active MgB / Al, amino coupling agent and deionized water are mixed in a flask, heated to 40-60°C and stirred for 3-6 hours, the reaction liquid is filtered to collect the solid, and the amination MgB / Al composite powder is obtained after washing and drying; S3, modification treatment: Dissolve bisphenol A diglycidyl ether in N,N-dimethylformamide, add amined MgB / Al composite powder, disperse evenly, heat to 60-80°C, stir for 6-12h, filter the reaction solution after the reaction is finished, collect the solid, wash and dry to obtain modified aluminum powder, i.e., reinforced filler; In S1, the ionic liquid [Bmim]BF4 is 1-butyl-3-methylimidazolium tetrafluoroborate, and the mass volume ratio of aluminum powder, magnesium acetate, anhydrous ethanol and ionic liquid [Bmim]BF4 is 1g:(0.14-0.28)g:(5-10)mL:(10-20)mL; the amount of sodium borohydride added is 10%-20% of the mass of magnesium acetate.
2. The silicon-free artificial stone according to claim 1, characterized in that: The unsaturated polyester resin is any one or more combinations of orthophthalic unsaturated polyester resin, isophthalic unsaturated polyester resin, and bisphenol A unsaturated polyester resin.
3. The silicon-free artificial stone according to claim 1, characterized in that: The curing agent is any one of 2-methyl ethyl peroxide, dibenzoyl peroxide and tert-butyl perbenzoate.
4. The silicon-free artificial stone according to claim 1, characterized in that: The pigment is an organic pigment, including one or more combinations of pigment yellow 139, pigment red 179, pigment blue 15, and pigment green 7.
5. The silicon-free artificial stone according to claim 1, characterized in that: During the preparation of the active MgB / Al of S2, the mass volume ratio of the MgB / Al composite powder and anhydrous ethanol is 1g:(10-20)mL; during the preparation of the amination MgB / Al composite powder of S2, the amino coupling agent is KH-550, and the mass volume ratio of the active MgB / Al, the amino coupling agent and deionized water is 1g:(0.2-0.3)g:(10-20)mL.
6. The silicon-free artificial stone according to claim 1, characterized in that: In S3, the mass ratio of the amino MgB / Al composite powder, bisphenol A diglycidyl ether and N,N-dimethylformamide is 1 g: (0.34-0.48) g: (10-20) mL.
7. A method for preparing the silicon-free artificial stone according to claim 1, characterized in that: The following steps are involved: (1) First, reinforcing filler, bamboo fiber and unsaturated polyester resin are mixed in a blender, and after stirring evenly, pigment and curing agent are added, and after stirring evenly again, a premix is obtained; (2) The premix is introduced into a mold, vibrated and degassed, pressed into shape, and then heated and cured to obtain a silicon-free artificial stone material.