A sand consolidating agent and its preparation method and application

By preparing sand solidifiers containing rich network structures and using static electricity and hydrogen bonding to fix the sand, the problem of poor adhesion performance of polyacrylic sand solidifiers is solved, high consolidation strength and high temperature resistance are achieved, and oil field production needs are met. .

CN118256219BActive Publication Date: 2024-11-22DONGYING CITY HAIJIA CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410410843.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2024-11-22
Estimated Expiration
2044-04-08

AI Technical Summary

Technical Problem

Polyacrylic sand fixing agents have problems such as poor bonding performance, low edge pressure strength and poor water retention performance in petroleum mining, soil restoration and treatment, and desert control, which limits their application.

Method used

By preparing a sand fixing agent, a rich network structure is formed by combining polypropionamide, polyacrylic acid, epoxy resin, phenolic resin, alkyl orthosilicate, aluminum isopropoxide, water, ethanol and ammonia water, using static electricity It acts and hydrogen bonds to fix the sand, and has good high temperature resistance and water retention properties.

Benefits of technology

It achieves high consolidation strength, high temperature resistance and good water absorption of sand solidifier, meets oil field production needs, and improves application effect and prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention proposes a sand consolidation agent and a preparation method and application thereof, and belongs to the technical field of oilfield sand consolidation. The sand consolidation agent is prepared by the following raw materials in parts by weight: 15-20 parts of polyacrylamide, 10-15 parts of polyacrylic acid, 3-5 parts of epoxy resin, 4-7 parts of phenolic resin, 7-10 parts of alkyl orthosilicate, 3-5 parts of aluminum isopropoxide, 20-30 parts of water, 15-30 parts of ethanol and 10-20 parts of ammonia water. The sand consolidation agent prepared by the present invention forms a rich network structure, contains rich hydroxyl groups, can be fixed with sand through electrostatic action and hydrogen bonding, and at the same time, has good high temperature resistance, water absorption and water retention, can fully meet the needs of oilfield production, and has good application effect and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oilfield sand consolidation, and in particular to a sand consolidation agent and a preparation method and application thereof. Background Art

[0002] Sand fixers are mainly used in the fields of oil extraction, soil remediation, desertification control, waterway regulation engineering, etc. There are mainly polyacrylic acid sand fixers, phenolic resin sand fixers, epoxy resin sand fixers, etc. Among them, polyacrylate sand fixers have the advantages of simple preparation method and low cost, and are widely used. However, polyacrylic acid sand fixers have poor adhesion to sand particles, low edge pressure strength, and poor water retention, which limits the application of polyacrylic acid sand fixers in the fields of oil extraction, soil remediation, desertification control, etc.

[0003] The problem of sand coming out of oil wells is widely present in oil extraction. It can lead to reduced oil well production, increased mining operation costs, damage to equipment and other problems. The usual way to solve the problem of sand coming out of oil wells is to inject sand-fixing agents to make the loose soil sand particles in the formation cemented and bonded, thereby achieving a sand-fixing effect. Summary of the invention

[0004] The purpose of the present invention is to propose a sand-fixing agent and a preparation method and application thereof. By forming a rich network structure, the structure contains rich hydroxyl groups and can be fixed to sand through electrostatic and hydrogen bonding. At the same time, it has good high temperature resistance and water absorption and water retention, can fully meet the needs of oil field production, and has good application effects and application prospects.

[0005] The technical solution of the present invention is achieved in this way:

[0006] The invention provides a sand consolidating agent, which is prepared from the following raw materials in parts by weight: 15-20 parts of polyacrylamide, 10-15 parts of polyacrylic acid, 3-5 parts of epoxy resin, 4-7 parts of phenolic resin, 7-10 parts of alkyl orthosilicate, 3-5 parts of aluminum isopropoxide, 20-30 parts of water, 15-30 parts of ethanol and 10-20 parts of ammonia water.

[0007] As a further improvement of the present invention, the alkyl orthosilicate is ethyl orthosilicate or methyl orthosilicate.

[0008] As a further improvement of the present invention, the epoxy resin is a mixture of E44 and E51, with a mass ratio of 10-15:7-10.

[0009] As a further improvement of the present invention, the phenolic resin is phenolic resin 2127.

[0010] As a further improvement of the present invention, the polyacrylic acid is at least one of polyacrylic acid 2000 and PL2142-3000.

[0011] As a further improvement of the present invention, the concentration of the ammonia water is 20-25wt%.

[0012] The present invention further protects a method for preparing the above-mentioned sand consolidating agent, comprising the following steps:

[0013] S1. Add alkyl orthosilicate and aluminum isopropoxide to ethanol and stir to mix well to obtain material A;

[0014] S2. Add polyacrylamide, polyacrylic acid, epoxy resin and phenolic resin to water, heat and mix well to obtain material B;

[0015] S3. Mix material A and material B evenly, add ammonia water, stir and mix evenly to prepare a sand consolidating agent.

[0016] As a further improvement of the present invention, the stirring and mixing time in step S1 is 20-30 minutes; and the stirring and mixing time in step S3 is 1-3 hours.

[0017] As a further improvement of the present invention, the heating temperature in step S2 is 40-50° C. and the heating time is 1-3 hours.

[0018] The present invention further protects the use of the above-mentioned sand-fixing agent in oil extraction, soil remediation and management, sand and desertification prevention and control, and waterway regulation projects.

[0019] The present invention has the following beneficial effects:

[0020] The present invention prepares silicon / aluminum sol by a sol-gel method, adds a variety of resin materials, including polyacrylamide, polyacrylic acid, epoxy resin, and phenolic resin, and forms a rich network structure. The structure contains rich hydroxyl groups and can be fixed with sand through electrostatic action and hydrogen bonding. At the same time, the structure has good high temperature resistance and water absorption and water retention, can fully meet the production needs of oil fields, and has good application effects and application prospects. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] This embodiment provides a method for preparing a sand consolidating agent, comprising the following steps:

[0024] S1. 7 parts by weight of ethyl orthosilicate, 3 parts by weight of aluminum isopropoxide were added to 15 parts by weight of ethanol and stirred for 20 min to obtain material A;

[0025] S2. 15 parts by weight of polyacrylamide, 10 parts by weight of polyacrylic acid 2000, 3 parts by weight of epoxy resin, and 4 parts by weight of phenolic resin 2127 were added to 20 parts by weight of water, heated to 40°C, and stirred for 1h to obtain material B;

[0026] S3 A and B materials were mixed, 10 parts by weight of 20wt% ammonia was added, and the mixture was stirred for 1h to obtain a sand consolidating agent;

[0027] The epoxy resin is a mixture of E44 and E51, with a mass ratio of 10:7.

[0028] Example 2

[0029] This embodiment provides a method for preparing a sand consolidating agent, comprising the following steps:

[0030] S1. 10 parts by weight of methyl orthosilicate, 5 parts by weight of aluminum isopropoxide were added to 30 parts by weight of ethanol and stirred for 30 min to obtain material A;

[0031] S2. 20 parts by weight of polyacrylamide, 15 parts by weight of polyacrylic acid PL2142-3000, 5 parts by weight of epoxy resin, and 7 parts by weight of phenolic resin 2127 were added to 30 parts by weight of water, heated to 50°C, and stirred for 3h to obtain material B;

[0032] S3 A and B materials were mixed, 20 parts by weight of 25wt% ammonia was added, and stirred for 3h to obtain a sand consolidation agent;

[0033] The epoxy resin is a mixture of E44 and E51, with a mass ratio of 15:10.

[0034] Example 3

[0035] This embodiment provides a method for preparing a sand consolidating agent, comprising the following steps:

[0036] S1. 8 parts by weight of ethyl orthosilicate, 4 parts by weight of aluminum isopropoxide were added to 22 parts by weight of ethanol and stirred for 25 min to obtain material A;

[0037] S2. 17 parts by weight of polyacrylamide, 12 parts by weight of polyacrylic acid 2000, 4 parts by weight of epoxy resin, and 6 parts by weight of phenolic resin 2127 were added to 25 parts by weight of water, heated to 45 ° C, stirred and mixed for 2h to obtain material B;

[0038] S3 A and B materials were mixed, 15 parts by weight of 22wt% ammonia was added, stirred and mixed for 2h to obtain a sand consolidation agent;

[0039] The epoxy resin is a mixture of E44 and E51, with a mass ratio of 12:8.

[0040] Comparative Example 1

[0041] The difference compared with Example 3 is that tetraethyl orthosilicate is not added.

[0042] The details are as follows:

[0043] S1. 12 parts by weight of aluminum isopropoxide was added to 22 parts by weight of ethanol and stirred for 25 min to obtain material A;

[0044] S2. 17 parts by weight of polyacrylamide, 12 parts by weight of polyacrylic acid 2000, 4 parts by weight of epoxy resin, and 6 parts by weight of phenolic resin 2127 were added to 25 parts by weight of water, heated to 45 ° C, stirred and mixed for 2h to obtain material B;

[0045] S3 A and B materials were mixed, 15 parts by weight of 22wt% ammonia was added, stirred and mixed for 2h to obtain a sand consolidation agent;

[0046] The epoxy resin is a mixture of E44 and E51, with a mass ratio of 12:8.

[0047] Comparative Example 2

[0048] The difference compared with Example 3 is that aluminum isopropoxide is not added.

[0049] The details are as follows:

[0050] S1. 12 parts by weight of ethyl orthosilicate was added to 22 parts by weight of ethanol and stirred for 25 min to obtain material A;

[0051] S2. 17 parts by weight of polyacrylamide, 12 parts by weight of polyacrylic acid 2000, 4 parts by weight of epoxy resin, and 6 parts by weight of phenolic resin 2127 were added to 25 parts by weight of water, heated to 45 ° C, stirred and mixed for 2h to obtain material B;

[0052] S3 A and B materials were mixed, 15 parts by weight of 22wt% ammonia was added, stirred and mixed for 2h to obtain a sand consolidation agent;

[0053] The epoxy resin is a mixture of E44 and E51, with a mass ratio of 12:8.

[0054] Test Example 1

[0055] The sand consolidating agents prepared in Examples 1-3 of the present invention and Comparative Examples 1-2 were subjected to performance tests, and the results are shown in Table 1.

[0056] Table 1

[0057]

[0058] It can be seen from the above table that the sand consolidating agents prepared in Examples 1-3 of the present invention have high consolidation strength, high temperature resistance, and good permeability after solidification.

[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A sand consolidating agent, characterized in that: The invention is prepared from the following raw materials in parts by weight: 15-20 parts of polyacrylamide, 10-15 parts of polyacrylic acid, 3-5 parts of epoxy resin, 4-7 parts of phenolic resin, 7-10 parts of ethyl orthosilicate or methyl orthosilicate, 3-5 parts of aluminum isopropoxide, 20-30 parts of water, 15-30 parts of ethanol and 10-20 parts of aqueous ammonia.

2. The sand consolidating agent according to claim 1, characterized in that: The epoxy resin is a mixture of E44 and E51, with a mass ratio of 10-15:7-10.

3. The sand consolidating agent according to claim 1, characterized in that: The phenolic resin is phenolic resin 2127.

4. The sand consolidating agent according to claim 1, characterized in that: The polyacrylic acid is at least one of polyacrylic acid 2000 and PL2142-3000.

5. The sand consolidating agent according to claim 1, characterized in that: The concentration of the ammonia water is 20-25wt%.

6. A method for preparing a sand consolidating agent according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Add alkyl orthosilicate and aluminum isopropoxide to ethanol and stir to mix well to obtain material A; S2. Add polyacrylamide, polyacrylic acid, epoxy resin and phenolic resin to water, heat and mix well to obtain material B; S3. Mix material A and material B evenly, add ammonia water, stir and mix evenly to prepare a sand consolidating agent.

7. The preparation method according to claim 6, characterized in that: The stirring and mixing time in step S1 is 20-30 minutes; the stirring and mixing time in step S3 is 1-3 hours.

8. The preparation method according to claim 6, characterized in that: The heating temperature in step S2 is 40-50° C. and the heating time is 1-3 h.

9. Use of the sand-fixing agent according to any one of claims 1 to 5 in oil production, soil remediation and management, sand and desertification prevention, and waterway regulation projects.