A forging process for high-strength titanium alloy bars

Through microwave preheating and repeated piercing combined with soft-clad forging, the problem of uneven structure and unstable performance of titanium alloy rods has been solved, and high-strength and efficient titanium alloy rods have been produced to meet the needs of aviation parts. Service Requirements.

CN118268491BActive Publication Date: 2024-10-29SHANDONG LIANGMA NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410634007.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-21
Publication Date
2024-10-29
Estimated Expiration
2044-05-21

AI Technical Summary

Technical Problem

The existing forging process of α/β titanium alloys results in uneven structure and incomplete recrystallization of titanium alloy products, resulting in a mismatch in strength and plasticity, which cannot meet the service requirements of aerospace parts, and the large specific surface area of ​​the forging blank results in heat loss. , tissue inhomogeneity and unstable performance.

Method used

After microwave preheating treatment, through repeated pier drawing combined with soft sheathing forging method, the forging temperature, fire times and deformation amount are controlled, multi-fire pier drawing forging is performed, and soft sheathing method is used in the initial and final forging stages, combined with Preheat first and then solid solution treatment, strictly control production conditions, including microwave preheating, homogenization heat treatment, multi-fire pier drawing forging and post-forging heat treatment.

Benefits of technology

It improves the structural uniformity and performance stability of titanium alloy rods, increases strength, reduces recrystallization, enhances the production efficiency of titanium alloy rods, and ensures product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118268491B_ABST
    Figure CN118268491B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of forging, and specifically to a forging process for high-strength titanium alloy bars. A forging process for high-strength titanium alloy bars, comprising the following steps: preheat treatment; blank forging; first forging step; second forging step; third forging step; fourth forging step; post-forging heat treatment. The present invention adopts repeated upsetting and drawing combined with soft-encapsulation forging method, by controlling the forging temperature, upsetting and drawing fire times, deformation amount and other parameters of each step, and adopting the soft-encapsulation method in the initial and final forging stages, it can prevent the forging blank from cooling too fast during the forging process, reduce the forging cold die structure, improve the structural uniformity of the forging, and reduce the recrystallization phenomenon. At the same time, multi-fire upsetting and drawing is conducive to breaking the internal structure of the ingot, avoiding insufficient dynamic recrystallization, thereby improving the performance stability of the forging, and further improving the strength of the titanium alloy bar.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of forging, and in particular to a forging process for a high-strength titanium alloy bar. Background Art

[0002] Titanium alloy is an alloy metal made of titanium and other metals. It has the characteristics of high strength, good corrosion resistance, high heat resistance, good low temperature performance, and high chemical activity. It is widely used in the aerospace field. With the development of the aviation industry, in order to meet the service requirements of aviation parts, higher requirements are put forward for titanium alloy bars in terms of uniformity of organization and strength.

[0003] Most of the existing forging processes for α / β titanium alloys are to first forge several times above the phase transformation point and then forge several times below the phase transformation point. The above forging process is likely to cause defects such as uneven structure and incomplete recrystallization in various parts of the titanium alloy products, resulting in anisotropy of the mechanical properties of the bars or final components, so that their strength and plasticity cannot be well matched, and ultimately cannot meet the service requirements; in addition, due to the large specific surface area of ​​the forging blank, heat is easily dissipated during the forging process, further leading to uneven structure and unstable performance of the titanium alloy bars. Therefore, in order to solve the above problems, it is urgently necessary to provide a forging process for high-strength titanium alloy bars. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention aims to provide a forging process for a high-strength titanium alloy bar.

[0005] A forging process for a high-strength titanium alloy bar comprises the following steps:

[0006] Step 1: Preheating

[0007] A titanium alloy ingot raw material is selected, subjected to microwave preheating treatment, and then transferred to a heating furnace for homogenization treatment to obtain a preheated titanium alloy ingot;

[0008] Step 2: Forging

[0009] The preheated titanium alloy ingot is forged by blanking, and then subjected to one fire, two punching and two drawing, the heating temperature is 20-40°C above the phase transformation point, the heating and holding time is 150-180min, the forging ratio of each fire is 1.5-2, and the hammer is pressed down at a uniform speed to obtain a primary forging blank;

[0010] Step 3, first forging step

[0011] The primary forging billet is subjected to two-time forging and drawing, all of which are soft-packed, the heating temperature of each time is 20-40°C below the phase transition point, the heating and holding time is 100-120min, the forging ratio is controlled between 1.3-1.8, and the hammer is pressed down at a uniform speed to obtain the first forging billet;

[0012] Step 4, Second Forging Step

[0013] The first forging billet is subjected to two-time upsetting forging, the heating temperature of each time is 40-60°C below the phase transformation point, and reversing upsetting, diagonal upsetting and upsetting are performed in sequence, and the heating and heat preservation time of each time is 100-120min, to obtain the second forging billet;

[0014] Step 5, the third forging step

[0015] The second forging billet is subjected to two-time upsetting and drawing forging, each time the billet is heated to 60-70°C below the phase transformation point, and chamfering and drawing are performed in sequence, and rounding and drawing are performed, the forging ratio is controlled at 1.2-1.9, and the heating and heat preservation time of each time is 100-120 minutes, to obtain the third forging billet;

[0016] Step 6, the fourth forging step

[0017] The third forging billet is subjected to two-time upsetting forging, all of which are soft-packed, the heating temperature of each time is 70-80°C below the phase transition point, the heating and holding time is 80-110min, the forging ratio is controlled between 1.5-2, the hammer is pressed down at a uniform speed, and air cooling or water quenching is adopted after forging to obtain the forging;

[0018] Step 7: Heat treatment after forging

[0019] The forgings are placed in a holding furnace, first preheated at 600-650℃ for 20-30min, then heated to 900-960℃ for solution treatment, water cooled, aged in a holding furnace at 800-980℃, and air cooled to obtain high-strength titanium alloy bars.

[0020] Furthermore, the microwave preheating treatment uses industrial microwave equipment with a frequency of 2450 MHz, a microwave preheating time of 45 s, a pre-pressing height of 60 mm, and a preheating power of 6×750 W.

[0021] Furthermore, the first forging step adopts direct upsetting, and the fourth forging step adopts two-upsetting and two-drawing.

[0022] Furthermore, the soft package material is 304 stainless steel or TC4 titanium alloy.

[0023] Furthermore, before each firing, an anti-oxidation coating is applied to the surface of the forging blank.

[0024] Furthermore, the deformation amount of each forging step is controlled at 20-30%, and the upsetting deformation amount of each step is an upsetting ratio of 1.1-1.5.

[0025] Furthermore, each forging step is subjected to air cooling or water quenching after forging.

[0026] Furthermore, the heating temperature of the homogenization treatment is set to 350-500°C above the β phase transformation point, and the temperature is kept for 20-40 hours; the heating temperature of the blank forging is set to 200-250°C below the phase transformation point, and the heating and heat preservation time is 60-90 minutes.

[0027] Furthermore, the titanium alloy ingot is obtained by vacuum consumable electrode arc furnace smelting or vacuum consumable electrode shell protection smelting process.

[0028] Furthermore, the heating coefficient of the post-forging heat treatment process is 1.5-2min / mm.

[0029] The beneficial effects achieved by the present invention are as follows: 1. The present invention adopts a repeated upsetting and drawing combined with a soft-packing forging method. By controlling the forging temperature, upsetting and drawing fire times, deformation amount and other parameters of each process step, and adopting a soft-packing method in the initial and final forging stages, it can prevent the forging blank from cooling down too quickly during the forging process, reduce the forging cold die structure, improve the structural uniformity of the forging, and reduce recrystallization. At the same time, multiple upsetting and drawing fire times are beneficial to breaking up the internal structure of the ingot and avoiding insufficient dynamic recrystallization, thereby improving the performance stability of the forging, and then improving the strength of the titanium alloy bar.

[0030] 2. The present invention can prevent the growth of low-magnification coarse grains of the forgings by preheating the forgings first and then performing solid solution treatment, which is beneficial to grain refinement, thereby improving the uniformity of the structure of the titanium alloy rod.

[0031] 3. The present invention uses microwave preheating and then homogenization treatment on the titanium alloy ingot, which can make the temperature distribution inside the ingot uniform, make the internal structure more uniform, and at the same time increase the heating rate and improve the production efficiency of titanium alloy bars.

[0032] 4. The present invention adopts the method of first subjecting the titanium alloy to homogenization heat treatment, then performing billet forging above the phase transformation point, and then performing multi-fire drawing forging below the phase transformation point, which can first reduce the influence of the cast grains on the subsequent processes.

[0033] 5. The present invention helps to ensure the product quality of titanium alloy bars by strictly controlling production conditions and forging blank shape variables. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The forging process of the high-strength titanium alloy bar used in the embodiment of the present invention is a flow chart. DETAILED DESCRIPTION

[0035] The present invention is further described in detail below in conjunction with specific embodiments.

[0036] Example 1: A forging process for a high-strength titanium alloy bar, such as Figure 1 As shown, the following steps are included:

[0037] Step 1: Preheating

[0038] The titanium alloy ingot raw material obtained by vacuum consumable electrode arc furnace smelting or vacuum consumable electrode shell protection smelting process is selected for microwave preheating treatment, using industrial microwave equipment with a frequency of 2450MHz, a microwave preheating time of 45s, a pre-pressing height of 60mm, and a preheating power of 6×750W; then it is transferred to a heating furnace for homogenization treatment, the heating temperature is set to 350°C above the β phase transformation point, and the temperature is kept for 30h to obtain a preheated titanium alloy ingot;

[0039] Step 2: Forging

[0040] The preheated titanium alloy ingot is subjected to billet forging, the billet heating temperature is 200°C below the phase transformation point, the heating and holding time is 80 minutes, one fire is performed, and then two piers and two draws are performed for one fire, the heating temperature is 20°C above the phase transformation point, the heating and holding time is 150 minutes, the forging ratio of each fire is 1.5, the hammer is pressed at a uniform speed, and air cooling or water quenching is performed after forging to obtain the primary forging billet;

[0041] Step 3, first forging step

[0042] The primary forging blank is directly upset for 2 times, and all the forging times are soft-packed. The heating temperature of each forging time is 20°C below the phase transition point, the heating and holding time is 100 minutes, the forging ratio is controlled between 1.3, the hammer is pressed down at a uniform speed, and air cooling or water quenching is adopted after forging to obtain the first forging blank;

[0043] Step 4, Second Forging Step

[0044] The first forging billet is subjected to two-time upsetting forging, the heating temperature of each time is 40°C below the phase transformation point, and reversing upsetting, diagonal upsetting and upsetting are performed in sequence, the heating and heat preservation time of each time is 100 minutes, and air cooling or water quenching is adopted after forging to obtain the second forging billet;

[0045] Step 5, the third forging step

[0046] The second forging billet is subjected to two-time upsetting and drawing forging, each time the billet is heated to 60°C below the phase transformation point, and then chamfering and drawing, rounding and drawing are performed in sequence, the forging ratio is controlled at 1.2, the heating and holding time for each time is 100 minutes, and air cooling or water quenching is performed after forging to obtain the third forging billet;

[0047] Step 6, the fourth forging step

[0048] The third forging billet is subjected to two fires, two piers and two draws, and all fires are soft-packed. The heating temperature of each fire is 70°C below the phase change point, the heating and holding time is 80 minutes, the forging ratio is controlled between 1.5, the hammer is pressed down at a uniform speed, and air cooling or water quenching is adopted after forging to obtain the forging;

[0049] Step 7: Heat treatment after forging

[0050] The forgings were placed in a holding furnace, preheated at 650°C for 20 min, then heated to 960°C for solution treatment, water cooled, and aged in a holding furnace at 800°C with a heating coefficient of 1.5 min / mm. The steel was then air cooled to obtain high-strength titanium alloy bars.

[0051] Before each firing, the surface of the forging blank is coated with an anti-oxidation coating; the soft bag is made of 304 stainless steel; and the deformation of each forging step is controlled within 20%.

[0052] Example 2: A forging process for a high-strength titanium alloy bar, such as Figure 1 As shown, the following steps are included:

[0053] Step 1: Preheating

[0054] The titanium alloy ingot raw material obtained by vacuum consumable electrode arc furnace smelting or vacuum consumable electrode shell protection smelting process is selected for microwave preheating treatment, using industrial microwave equipment with a frequency of 2450MHz, a microwave preheating time of 45s, a pre-pressing height of 60mm, and a preheating power of 6×750W; then it is transferred to a heating furnace for homogenization treatment, the heating temperature is set to 450°C above the β phase transformation point, and the temperature is kept for 35h to obtain a preheated titanium alloy ingot;

[0055] Step 2: Forging

[0056] The preheated titanium alloy ingot is subjected to billet forging, the billet heating temperature is 250°C below the phase transformation point, the heating and holding time is 90 minutes, one fire is performed, and then two piers and two draws are performed for one fire, the heating temperature is 30°C above the phase transformation point, the heating and holding time is 160 minutes, the forging ratio of each fire is 1.5, the hammer is pressed at a uniform speed, and air cooling or water quenching is performed after forging to obtain the primary forging billet;

[0057] Step 3, first forging step

[0058] The primary forging blank is directly upset for 2 times, and all the forging times are soft-packed. The heating temperature of each forging time is 30℃ below the phase transition point, the heating and holding time is 120min, the forging ratio is controlled between 1.3, the hammer is pressed down at a uniform speed, and air cooling or water quenching is adopted after forging to obtain the first forging blank;

[0059] Step 4, Second Forging Step

[0060] The first forging billet is subjected to two-time upsetting forging, the heating temperature of each time is 50°C below the phase transformation point, and reversing upsetting, diagonal upsetting and upsetting are performed in sequence, the heating and heat preservation time of each time is 120min, and air cooling or water quenching is adopted after forging to obtain the second forging billet;

[0061] Step 5, the third forging step

[0062] The second forging billet is subjected to two-time upsetting and drawing forging, each time the billet is heated to 70°C below the phase transformation point, and then chamfering and drawing, rounding and drawing are performed in sequence, the forging ratio is controlled at 1.2, the heating and holding time for each time is 120 minutes, and air cooling or water quenching is performed after forging to obtain the third forging billet;

[0063] Step 6, the fourth forging step

[0064] The third forging blank is subjected to two fires, two piers and two draws, and all fires are soft-packed. The heating temperature of each fire is 80°C below the phase change point, the heating and holding time is 100 minutes, the forging ratio is controlled between 1.5, the hammer is pressed down at a uniform speed, and air cooling or water quenching is adopted after forging to obtain the forging;

[0065] Step 7: Heat treatment after forging

[0066] The forgings were placed in a holding furnace, preheated at 600°C for 30 minutes, then heated to 900°C for solution treatment, water-cooled, and aged in a holding furnace at 900°C with a heating coefficient of 2min / mm. The high-strength titanium alloy rods were obtained by air cooling.

[0067] Before each firing, the surface of the forging blank is coated with an anti-oxidation coating; the soft bag is made of 304 stainless steel; and the deformation of each forging step is controlled within 20%.

[0068] Example 3: A forging process for a high-strength titanium alloy bar, such as Figure 1 As shown, the following steps are included:

[0069] Step 1: Preheating

[0070] The titanium alloy ingot raw material obtained by vacuum consumable electrode arc furnace smelting or vacuum consumable electrode shell protection smelting process is selected for microwave preheating treatment, using industrial microwave equipment with a frequency of 2450MHz, a microwave preheating time of 45s, a pre-pressing height of 60mm, and a preheating power of 6×750W; then it is transferred to a heating furnace for homogenization treatment, the heating temperature is set to 350°C above the β phase transformation point, and the temperature is kept for 30h to obtain a preheated titanium alloy ingot;

[0071] Step 2: Forging

[0072] The preheated titanium alloy ingot is subjected to billet forging, the billet heating temperature is 200°C below the phase transformation point, the heating and holding time is 80 minutes, one fire is performed, and then two piers and two pulls are performed for one fire, the heating temperature is 20°C above the phase transformation point, the heating and holding time is 150 minutes, the forging ratio of each fire is 2, the hammer is pressed down at a uniform speed, and air cooling or water quenching is performed after forging to obtain the primary forging billet;

[0073] Step 3, first forging step

[0074] The primary forging blank is directly upset for 2 times, and all the forging times are soft-packed. The heating temperature of each forging time is 20℃ below the phase transition point, the heating and holding time is 100minmin, the forging ratio is controlled between 1.8, the hammer is pressed down at a uniform speed, and air cooling or water quenching is adopted after forging to obtain the first forging blank;

[0075] Step 4, Second Forging Step

[0076] The first forging billet is subjected to two-time upsetting forging, the heating temperature of each time is 40°C below the phase transformation point, and reversing upsetting, diagonal upsetting and upsetting are performed in sequence, the heating and heat preservation time of each time is 100 minutes, and air cooling or water quenching is adopted after forging to obtain the second forging billet;

[0077] Step 5, the third forging step

[0078] The second forging billet is subjected to two-time upsetting and drawing forging, each time the billet is heated to 60°C below the phase transformation point, and then chamfering and drawing, rounding and drawing are performed in sequence, the forging ratio is controlled at 1.5, the heating and holding time for each time is 100 minutes, and air cooling or water quenching is performed after forging to obtain the third forging billet;

[0079] Step 6, the fourth forging step

[0080] The third forging billet is subjected to two fires, two piers and two draws, and all fires are soft-packed. The heating temperature of each fire is 70°C below the phase change point, the heating and holding time is 80 minutes, the forging ratio is controlled between 2, the hammer is pressed down at a uniform speed, and air cooling or water quenching is adopted after forging to obtain the forging;

[0081] Step 7: Heat treatment after forging

[0082] The forgings were placed in a holding furnace, preheated at 650°C for 20 min, then heated to 960°C for solution treatment, water cooled, and aged in a holding furnace at 800°C with a heating coefficient of 1.5 min / mm. The steel was then air cooled to obtain high-strength titanium alloy bars.

[0083] Before each firing, the surface of the forging blank is coated with an anti-oxidation coating; the soft bag is made of 304 stainless steel; and the deformation of each forging step is controlled within 25%.

[0084] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A forging process for a high-strength titanium alloy bar, characterized in that: The following steps are involved: Step 1: Preheating A titanium alloy ingot raw material is selected, subjected to microwave preheating treatment, and then transferred to a heating furnace for homogenization treatment to obtain a preheated titanium alloy ingot; Step 2: Forging The preheated titanium alloy ingot is forged by blanking, and then subjected to one fire, two punching and two drawing, the heating temperature is 20-40°C above the phase transformation point, the heating and holding time is 150-180min, the forging ratio of each fire is 1.5-2, and the hammer is pressed down at a uniform speed to obtain a primary forging blank; Step 3, first forging step The primary forging billet is subjected to two-time forging and drawing, all of which are soft-packed, the heating temperature of each time is 20-40°C below the phase transition point, the heating and holding time is 100-120min, the forging ratio is controlled between 1.3-1.8, and the hammer is pressed down at a uniform speed to obtain the first forging billet; Step 4, Second Forging Step The first forging billet is subjected to two-time upsetting forging, the heating temperature of each time is 40-60°C below the phase transformation point, and reversing upsetting, diagonal upsetting and upsetting are performed in sequence, the heating and heat preservation time of each time is 100-120min, and air cooling or water quenching is performed after forging to obtain the second forging billet; Step 5, the third forging step The second forging billet is subjected to two-time upsetting and drawing forging, each time the billet is heated to 60-70°C below the phase transformation point, and chamfering and drawing are performed in sequence, and rounding and drawing are performed, the forging ratio is controlled at 1.2-1.9, and the heating and heat preservation time of each time is 100-120 minutes, to obtain the third forging billet; Step 6, the fourth forging step The third forging billet is subjected to two-time forging and drawing, all of which are soft-packed, the heating temperature of each time is 70-80°C below the phase change point, the heating and holding time is 80-110min, the forging ratio is controlled between 1.5-2, and the hammer is pressed down at a uniform speed to obtain the forging; Step 7: Heat treatment after forging The forgings are placed in a holding furnace, first preheated at 600-650℃ for 20-30min, then heated to 900-960℃ for solution treatment, water cooled, aged in a holding furnace at 800-980℃, and air cooled to obtain high-strength titanium alloy bars.

2. A forging process for a high-strength titanium alloy bar according to claim 1, characterized in that: The microwave preheating treatment uses industrial microwave equipment with a frequency of 2450 MHz, a microwave preheating time of 45 seconds, a pre-pressing height of 60 mm, and a preheating power of 6×750 W.

3. The forging process of a high-strength titanium alloy bar according to claim 1, characterized in that: The first forging step adopts direct upsetting, and the fourth forging step adopts two-piercing and two-drawing.

4. The forging process of a high-strength titanium alloy bar according to claim 1, characterized in that: The soft package is made of 304 stainless steel or TC4 titanium alloy.

5. The forging process of a high-strength titanium alloy bar according to claim 1, characterized in that: Before each firing, an anti-oxidation coating is applied to the surface of the forging blank.

6. The forging process of a high-strength titanium alloy bar according to claim 1, characterized in that: The deformation amount of each forging step is controlled at 20-30%, and the upsetting deformation amount of each step is an upsetting ratio of 1.1-1.

5.

7. The forging process of a high-strength titanium alloy bar according to claim 1, characterized in that: Each forging step is air-cooled or water-quenched after forging.

8. The forging process of a high-strength titanium alloy bar according to claim 1, characterized in that: The heating temperature of the homogenization treatment is set to 350-500°C above the β phase transformation point, and the temperature is kept for 20-40 hours; the heating temperature of the blank forging is set to 200-250°C below the phase transformation point, and the heating and heat preservation time is 60-90 minutes.

9. The forging process of a high-strength titanium alloy bar according to claim 1, characterized in that: The titanium alloy ingot is obtained by vacuum consumable electrode arc furnace smelting or vacuum consumable electrode shell protection smelting process.

10. The forging process of a high-strength titanium alloy bar according to claim 1, characterized in that: The heating coefficient of the post-forging heat treatment process is 1.5-2 min / mm.

Citation Information

Patent Citations

  • Forging method for TC17 titanium alloy beta

    CN111036832A

  • Forging method for Ti17 titanium alloy large-specification bar with high structure uniformity

    CN115595521A