Aluminum alloy material capable of delaying natural aging process and preparation method thereof

By using specific alloy components and process flows in aluminum alloys, the natural aging process of aluminum alloys is delayed, the fracture problem of aluminum alloys caused by natural age hardening after quenching is solved, the yield and processing stability are improved, and the flattening time is prolonged. No cracking time.

CN118272708BActive Publication Date: 2024-10-15SUZHOU RIZHONGTIAN ALUMINUM CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410711339.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-15
Estimated Expiration
2044-06-04

Smart Images

  • Figure CN118272708B_ABST
    Figure CN118272708B_ABST
Patent Text Reader

Abstract

An aluminum alloy material capable of delaying the natural aging process and a preparation method thereof, comprising the following components in mass percentage: Si 0.4-0.8%, Mg 0.8-1.2%, Fe≤0.15%, Cu 0.3-0.60%, Mn 0.04-0.08%, Cr 0.04-0.08%, Sn 0.04-0.08%, In≤0.04%, Zr 0.09-0.13%, Ti≤0.03%, Zn≤0.02%, the balance being Al, and a single impurity element≤0.05%. The present invention adopts a multi-stage homogenization process in the preparation process through reasonable alloy component ratio and micro-alloying treatment; the storage time after homogenization exceeds 30 days, and a short-time heating process is added; the extrusion online cooling rate is controlled; and at the same time, the relationship between the storage time before flattening and the air temperature during flattening is reasonably matched to obtain an aluminum alloy and a preparation method that can delay the natural aging process, thereby solving the problems of flattening fracture, cracking, etc. that traditional aluminum alloys will appear after being parked for a short time after quenching.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nonferrous metals, and in particular to an aluminum alloy material capable of delaying the natural aging process and a preparation method thereof. Background Art

[0002] Aluminum alloys have been widely used and developed in the fields of rail transit, aerospace, 5G communications, high-end ladders, etc. due to their high specific strength, good plasticity, excellent formability and corrosion resistance. However, with the increase in the application of aluminum alloys, the subsequent deep processing of aluminum alloy profiles is no longer a simple processing form with constant cross-sectional dimensions such as sawing, milling, and drilling. More and more processing methods that change the cross-section are being used, such as stretching, bending, flattening, and stamping. In order to better exert the plasticity of the material, these processes are generally carried out after the aluminum profile is hot extruded and quenched online, and then aged after processing, commonly known as "post-aging."

[0003] After hot extrusion of aluminum alloy, the solute atoms are dissolved in the matrix and are in a soft state. At this time, if it can be stretched, bent, flattened and processed immediately, the formability is good and the yield rate is high. However, due to the inevitable storage of aluminum profiles after quenching, such as transportation, turnover, and precision cutting, it is impossible to achieve immediate processing. It is well known that aluminum alloys after quenching have a natural aging hardening effect. The strength of the material increases rapidly during the storage process, and the elongation drops sharply, resulting in an increase in the proportion of fractures and cracks during the processing, which seriously affects the yield rate of the material.

[0004] In response to this problem, some domestic and foreign companies have also developed some materials and processes, such as the "Retrograde Heat Treatment" process in "Progress in Retrograde Heat Treatment of Aluminum Alloys and New Applications" and U.S. Patent US7996978B2. It requires the use of special equipment to perform local retrograde heat treatment on the material, which not only increases the equipment and processes, but also increases the cost of the material.

[0005] Therefore, it is of great significance to develop an aluminum alloy material and a production method thereof that can delay the natural aging process. Summary of the invention

[0006] The object of the present invention is to provide an aluminum alloy material capable of delaying the natural aging process and a preparation method thereof.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is: an aluminum alloy material capable of delaying the natural aging process, comprising the following components in mass percentage:

[0008] Si 0.4-0.8%, Mg 0.8-1.2%, Fe≤0.15%, Cu 0.3-0.60%, Mn 0.04-0.08%, Cr0.04-0.08%, Sn 0.04-0.08%, In≤ 0.04%, Zr 0.09-0.13%, Ti≤0.03%, Zn ≤0.02%, the balance is Al, and a single impurity element is ≤0.05%.

[0009] The present invention also provides a method for preparing an aluminum alloy material capable of delaying the natural aging process, comprising the following steps:

[0010] The following steps are involved:

[0011] S1: The ingredients are prepared according to the following mass percentages: Si 0.4-0.8%, Mg 0.8-1.2%, Fe≤0.15%, Cu0.3-0.60%, Mn 0.04-0.08%, Cr 0.04-0.08%, Sn 0.04-0.08%, In≤ 0.04%, Zr 0.09-0.13%, Ti≤0.03%, Zn ≤0.02%, the balance is Al, and a single impurity element is ≤0.05%, wherein aluminum is aluminum ingot, magnesium is magnesium ingot, and other elements are intermediate alloys; the prepared raw materials are heated, melted, stirred, refined, slag-scraped, allowed to stand, degassed online, filtered, and cast to obtain aluminum alloy round ingots;

[0012] S2: Perform multi-stage homogenization annealing on the aluminum alloy round ingot: heat up from room temperature to 420±5°C at a heating rate of 90°C / h, keep warm for 3-5 hours, then heat up to 530±5°C at a heating rate of 35°C / h, keep warm for 4-6 hours, then heat up to 570±5°C at a heating rate of 35°C / h, keep warm for 7-9 hours, then quickly cool to room temperature to obtain a homogenized aluminum alloy round bar A, which is then placed;

[0013] S3: When the placement time of the aluminum alloy round bar A in S2 is greater than 30 days, short-term heating is performed, the temperature is raised from room temperature to 560±5°C at a heating rate of 90°C / h, and the temperature is kept for 2 hours, and then the aluminum alloy round bar B is obtained by rapid cooling; when the placement time of the aluminum alloy round bar A is less than or equal to 30 days, the step S4 is directly performed;

[0014] S4: heating and extruding the aluminum alloy round bar A or B to obtain a profile, and performing online quenching on the extruded profile. The online quenching adopts strong wind cooling quenching, and the cooling rate of the profile in the temperature range from extrusion to cooling to 200° C. is 12-15° C. / s;

[0015] S5: After the profile is cooled down to room temperature online, it is straightened and flattened: when the room temperature is 5±5℃, the straightened profile is flattened within 285h; when the room temperature is 15±5℃, the straightened profile is flattened within 144h; when the room temperature is 25±5℃, the straightened profile is flattened within 50h; when the room temperature is 35±5℃, the straightened profile is flattened within 23h;

[0016] S6: The flattened profile of S5 is aged in an aging furnace at a temperature of 180±3℃ and a holding time of 4h.

[0017] The relevant contents in the above technical solution are explained as follows:

[0018] 1. In the above scheme, in S1, the Mg / Si ratio is controlled between 1 and 2.4.

[0019] 2. In the above scheme, in S1, the heating and melting temperature is 700-800°C.

[0020] 3. In the above scheme, in S1, the aluminum alloy melt obtained after standing is transferred into a flow channel. During the flow channel transfer process, a grain refiner is added to the flow channel, and then online degassing and filtering are performed.

[0021] 4. In the above solution, the grain refiner is an aluminum-titanium-boron grain refiner.

[0022] 5. In the above scheme, in S4, the heating temperature is 450-550°C.

[0023] 6. In the above scheme, in S4, the extrusion speed is 3.6-4.5 mm / s, and the outlet temperature of the front beam of the extrusion is ≥525°C.

[0024] 7. In the above solution, in S5, the straightness of the profile after straightening is ≤0.5mm / m.

[0025] The design principle and technical effects of the present invention are as follows:

[0026] The inventors of the present invention, through a lot of creative work, have achieved a reasonable alloy composition ratio and micro-alloying treatment, adopted a multi-stage homogenization treatment process in the preparation process; the placement time after homogenization exceeded 30 days, and a short-time heating process was added; the extrusion online cooling rate was controlled; and at the same time, the relationship between the placement time before flattening and the air temperature during flattening was reasonably matched to obtain an aluminum alloy and a preparation method that can delay the natural aging process, which solves the problems of flattening fracture and cracking that occur when traditional aluminum alloys are placed for a short time after quenching.

[0027] 1. The present invention reasonably controls the Mg / Si ratio between 1 and 2.4, and the total amount of Mg2Si between 1.2 and 1.9%, which can not only ensure the strength of the final material after aging, but also delay the natural aging process of the aluminum alloy.

[0028] 2. In traditional aluminum alloys, vacancies preferentially form vacancy pairs with MgSi clusters, resulting in a very fast natural aging process of aluminum alloys. In the technical solution of the present invention, after adding Sn and In elements, Sn and In capture a large number of supersaturated vacancies during the extrusion quenching cooling process, reducing the rapid precipitation process of MgSi clusters through vacancies and delaying the natural aging process.

[0029] 3. The technical solution of the present invention particularly emphasizes the control of the cooling rate during extrusion. When the cooling rate is too slow, the strength of the profile will decrease significantly, while when the rate is too fast, the effect of delaying natural aging will be weakened.

[0030] 4. When the profile is placed at 0-40℃, when the temperature is low (such as winter), it will not crack even if it is flattened for a long time (for example: 285h). As the placement temperature increases, the pinning effect of Sn and In on vacancies decreases rapidly, and the effect of delaying natural aging weakens, and the flattening time without cracking becomes significantly shorter (23h). However, compared with the traditional 6061 alloy, after adding Sn and In elements, the flattening time without cracking is extended by 4-5 times (for example, from 5-6h to more than 20h). BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Attached Figure 1 The curve of the change of the Vickers hardness of the profile after extrusion versus the placement time in the embodiment of the present invention;

[0032] Attached Figure 2 Table 3 is a classification diagram of stamping products of the present invention (from left to right, 1 to 5 respectively). DETAILED DESCRIPTION

[0033] The present invention is further described in detail below in conjunction with examples, and the embodiments of the present invention include but are not limited to these.

[0034] Embodiment 1: In this embodiment, an aluminum alloy capable of delaying the natural aging process is prepared, and the weight percentage of each element in its composition is Mg 1.05%, Si 0.66%, Fe 0.12%, Cu 0.36%, Mn 0.05%, Cr 0.04%, Sn 0.05%, In 0.01%, Zn 0.01%, Zr 0.1%, Ti 0.02%, and the balance is Al for material preparation, and a single impurity element is ≤0.05%.

[0035] The raw materials used to prepare the above Al-Mg-Si alloy are as follows:

[0036] Aluminum ingot: Aluminum ingot with the grade of Al99.7 in accordance with GB / T 1196-2008 is used, and the mass percentage of Al in the ingot is not less than 99.7%;

[0037] Magnesium ingot: Use magnesium ingot with the grade of Mg9990 in accordance with GB / T 3499-2003, and the mass percentage of Mg in the magnesium ingot shall not be less than 99.9%;

[0038] Master alloy: aluminum-based master alloys of grades AlSi20 and AlB3 that comply with YS / T 282-2000 are used, and the rare earth master alloy uses commercially available AlIn10 alloy.

[0039] The above raw materials are melted, cast, extruded and processed to obtain the profile of Example 1 and the semi-finished aluminum alloy ladder treads thereof. The specific steps and parameters are as follows:

[0040] The above raw materials are put into a tilting melting and holding furnace in proportion, and natural gas is used as the raw material to heat to 740°C for melting, and then AlB3 and AlIn10 master alloys are added to the melt, and electromagnetic stirring is performed for 20 minutes. Then, the melt is refined, degassed, and slag-stripped, and the temperature is adjusted and then allowed to stand for 30 to 40 minutes to obtain a melt;

[0041] (2) During the launder transfer process, a high-grade (Grade A) aluminum-titanium-boron grain refiner is added to the launder, followed by an online degassing and filtration device, where a 40+80 PPI dual-stage ceramic foam filter plate is used;

[0042] (3) semi-continuously casting the melt obtained in (2) at 730° C., using an “oil-gas sliding” crystallizer to control the surface quality of the ingot and the metallurgical quality of the cast rod, to obtain an aluminum alloy round ingot;

[0043] (4) subjecting the aluminum alloy round ingot obtained in (3) to homogenization annealing, heating from room temperature to 420±5°C at a heating rate of 90°C / h, keeping the temperature for 4 hours, then heating to 530±5°C at a heating rate of 35°C / h, keeping the temperature for 5 hours, then heating to 570±5°C at a heating rate of 35°C / h again, keeping the temperature for 8 hours, and then rapidly cooling to room temperature;

[0044] (5) The round ingot obtained in (4) is heated to 470-510°C and then extruded into a profile. The extrusion ratio is 42, the extrusion speed is 3.6-4.5 mm / s, and the profile temperature at the exit of the beam before extrusion is 525°C. After extrusion, the profile is cooled online with weak wind at a cooling rate of 13°C / s and cut to size to obtain the profile.

[0045] (6) The profile obtained in (5) is subjected to step stamping processing.

[0046] (7) The intermediate product obtained after the step stamping process was subjected to aging treatment at a temperature of 180°C for 4 h. The mechanical properties were measured after aging.

[0047] The air temperature during extrusion is 5±5°C, and the extrusion time is 7 days after the casting rod is homogenized.

[0048] Embodiment 2: In this embodiment, an aluminum alloy capable of delaying the natural aging process is prepared, and the weight percentage of each element in its composition is Mg 1.05%, Si 0.66%, Fe 0.12%, Cu 0.36%, Mn 0.05%, Cr 0.04%, Sn 0.05%, In0.01%, Zn 0.01%, Zr 0.1%, Ti 0.02%, and the balance is Al for material preparation, and a single impurity element is ≤0.05%.

[0049] The raw materials, implementation steps, homogenization treatment system, extrusion parameters, online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0050] However, the extrusion time was controlled to be 7 days after the casting rod was homogenized, and the air temperature during extrusion was 15±5℃.

[0051] Embodiment 3: In this embodiment, an aluminum alloy capable of delaying the natural aging process is prepared, and the weight percentage of each element in its composition is Mg 1.05%, Si 0.66%, Fe 0.12%, Cu 0.36%, Mn 0.05%, Cr 0.04%, Sn 0.05%, In0.01%, Zn 0.01%, Zr 0.1%, Ti 0.02%, and the balance is Al for material preparation, and a single impurity element is ≤0.05%.

[0052] The raw materials, implementation steps, homogenization treatment system, extrusion parameters (cooling rate after extrusion 12°C / s), online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0053] However, the extrusion time was controlled to be 7 days after the casting rod was homogenized, and the air temperature during extrusion was 25±5℃.

[0054] Embodiment 4: In this embodiment, an aluminum alloy capable of delaying the natural aging process is prepared, and the weight percentage of each element in its composition is Mg 1.05%, Si 0.66%, Fe 0.12%, Cu 0.36%, Mn 0.05%, Cr 0.04%, Sn 0.05%, In0.01%, Zn 0.01%, Zr 0.1%, Ti 0.02%, and the balance is Al for material preparation, and a single impurity element is ≤0.05%.

[0055] The raw materials, implementation steps, homogenization treatment system, extrusion parameters (cooling rate after extrusion 14°C / s), online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0056] However, the extrusion time was controlled to be 7 days after the casting rod was homogenized, and the air temperature during extrusion was 35±5℃.

[0057] Embodiment 5: In this embodiment, an aluminum alloy capable of delaying the natural aging process is prepared, and the weight percentage of each element in its composition is Mg 1.05%, Si 0.66%, Fe 0.12%, Cu 0.36%, Mn 0.05%, Cr 0.04%, Sn 0.05%, In0.01%, Zn 0.01%, Zr 0.1%, Ti 0.02%, and the balance is Al for material preparation, and a single impurity element is ≤0.05%.

[0058] The raw materials, implementation steps, homogenization treatment system, extrusion parameters, online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0059] However, the extrusion time is controlled to be 25 days after the casting rod is homogenized, and the air temperature during extrusion is 25±5℃.

[0060] Embodiment 6: In this embodiment, an aluminum alloy capable of delaying the natural aging process is prepared, and the weight percentage of each element in its composition is Mg 1.05%, Si 0.66%, Fe 0.12%, Cu 0.36%, Mn 0.05%, Cr 0.04%, Sn 0.05%, In0.01%, Zn 0.01%, Zr 0.1%, Ti 0.02%, and the balance is Al for material preparation, and a single impurity element is ≤0.05%.

[0061] The raw materials, implementation steps, homogenization treatment system, extrusion parameters (cooling rate after extrusion 15°C / s), online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0062] However, the extrusion time is controlled to be 100 days after the homogenization treatment of the cast rods, and the cast rods are subjected to short-term heating treatment before extrusion. The short-term heating treatment system is to heat the rods from room temperature to 560±5℃ at a heating rate of 90℃ / h, keep the temperature for 2 hours, and then quickly cool to room temperature. The air temperature during extrusion is 25±5℃.

[0063] Example 7: In this example, an aluminum alloy capable of delaying the natural aging process is prepared, and the weight percentage of each element in its composition is Mg 1.05%, Si 0.66%, Fe 0.12%, Cu 0.36%, Mn 0.05%, Cr 0.04%, Sn 0.04%, In 0.04%, Zn 0.01%, Zr 0.1%, Ti 0.02%, and the balance is Al for preparation, and a single impurity element is ≤0.05%.

[0064] The raw materials, implementation steps, homogenization treatment system, extrusion parameters, online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0065] However, the extrusion time was controlled to be 7 days after the casting rod was homogenized, and the air temperature during extrusion was 25±5℃.

[0066] Example 8: In this example, an aluminum alloy capable of delaying the natural aging process is prepared, and the weight percentage of each element in its composition is Mg 1.2%, Si 0.70%, Fe 0.12%, Cu 0.56%, Mn 0.05%, Cr 0.04%, Sn 0.04%, In 0.01%, Zn 0.01%, Zr 0.0.11%, Ti 0.02%, and the balance is Al for preparation, and a single impurity element is ≤0.05%.

[0067] The raw materials, implementation steps, homogenization treatment system, extrusion parameters, online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0068] However, the extrusion time was controlled to be 7 days after the casting rod was homogenized, and the air temperature during extrusion was 25±5℃.

[0069] Comparative Example 1:

[0070] This comparative example is prepared according to the composition requirements of 6061 alloy in the national standard, and the weight percentage of each element is Si 0.64%, Mg 1.16%, Fe 0.16%, Cu 0.34%, Mn 0.08%, Cr 0.08%, Zn 0.02%, Ti 0.03%, and the balance is Al for batching, and a single impurity element is ≤0.05%.

[0071] The raw materials, implementation steps, homogenization treatment system, extrusion parameters, online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0072] However, the extrusion time was controlled to be 7 days after the casting rod was homogenized, and the air temperature during extrusion was 5±5℃.

[0073] Comparative Example 2:

[0074] This comparative example is prepared according to the composition requirements of 6061 alloy in the national standard, and the weight percentage of each element is Si 0.64%, Mg 1.16%, Fe 0.16%, Cu 0.34%, Mn 0.08%, Cr 0.08%, Zn 0.02%, Ti 0.03%, and the balance is Al for batching, and a single impurity element is ≤0.05%.

[0075] The raw materials, implementation steps, homogenization treatment system, extrusion parameters, online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0076] However, the extrusion time was controlled to be 7 days after the casting rod was homogenized, and the air temperature during extrusion was 15±5℃.

[0077] Comparative Example 3:

[0078] This comparative example is prepared according to the composition requirements of 6061 alloy in the national standard, and the weight percentage of each element is Si 0.64%, Mg 1.16%, Fe 0.16%, Cu 0.34%, Mn 0.08%, Cr 0.08%, Zn 0.02%, Ti 0.03%, and the balance is Al for batching, and a single impurity element is ≤0.05%.

[0079] The raw materials, implementation steps, homogenization treatment system, extrusion parameters, online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0080] However, the extrusion time was controlled to be 7 days after the casting rod was homogenized, and the air temperature during extrusion was 25±5℃.

[0081] Comparative Example 4:

[0082] This comparative example is prepared according to the composition requirements of 6061 alloy in the national standard, and the weight percentage of each element is Si 0.64%, Mg 1.16%, Fe 0.16%, Cu 0.34%, Mn 0.08%, Cr 0.08%, Zn 0.02%, Ti 0.03%, and the balance is Al for batching, and a single impurity element is ≤0.05%.

[0083] The raw materials, implementation steps, homogenization treatment system, extrusion parameters, online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0084] However, the extrusion time was controlled to be 7 days after the casting rod was homogenized, and the air temperature during extrusion was 35±5℃.

[0085] Comparative Example 5:

[0086] In this embodiment, an aluminum alloy capable of delaying the natural aging process is prepared, and the weight percentage of each element in the aluminum alloy composition is Mg 1.05%, Si 0.66%, Fe 0.12%, Cu 0.36%, Mn 0.05%, Cr 0.04%, Sn 0.05%, In0.01%, Zn 0.01%, Zr 0.1%, Ti 0.02%, and the balance is Al for material preparation, and a single impurity element is ≤0.05%.

[0087] The raw materials, implementation steps, homogenization treatment system, extrusion parameters, online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0088] However, the extrusion time was controlled to be 35 days after the casting rod was homogenized, and the air temperature during extrusion was 25±5℃.

[0089] Comparative Example 6:

[0090] In this embodiment, an aluminum alloy capable of delaying the natural aging process is prepared, and the weight percentage of each element in the aluminum alloy composition is Mg 1.05%, Si 0.66%, Fe 0.12%, Cu 0.36%, Mn 0.05%, Cr 0.04%, Sn 0.05%, In0.01%, Zn 0.01%, Zr 0.1%, Ti 0.02%, and the balance is Al for material preparation, and a single impurity element is ≤0.05%.

[0091] The raw materials, implementation steps, homogenization treatment system, extrusion parameters, online straightening parameters and aging treatment system selected during melting and casting are the same as those in Example 1.

[0092] However, the extrusion time is controlled to be 100 days after the casting rod is homogenized, and the air temperature during extrusion is 25±5℃.

[0093] The materials and aluminum alloy ladder tread intermediate products obtained in the above-mentioned Examples 1-8 and Comparative Examples 1-6 were subjected to the following tests and analyses:

[0094] 1. Carry out mechanical property tests in accordance with GB / T228.1-2021 "Tensile test of metallic materials - Part 1: Room temperature specimen method";

[0095] 2. Long-term continuous Webster hardness measurement and hardness curve drawing;

[0096] Among them, the above-mentioned Webster hardness determination method is to use the Webster hardness tester to accurately read the hardness of the measured product: clean the surface of the measured sample, keep it flat, and keep it vertical to the indenter. The bottom of the sample is in linear contact with the anvil. At a distance of more than 5mm from the edge, use the Webster hardness tester to measure the hardness. Specific operation: hold the movable handle tightly and clamp the profile until you feel that it has been pressed to the bottom. The pointer on the meter head points to a reading, which is the measured hardness value;

[0097] 3. Long-term continuous stamping and flattening processing test and stamping grade classification;

[0098] The specific method of the above-mentioned continuous stamping and flattening processing test is to use the MT-2IAAL external step flattening and cutting equipment to perform the profile step flattening cracking test, place the extruded profile in the stamping die, step on the operating pedal, and after stamping and cutting, leave the pedal, use professional tools to remove the residual material, observe whether there are cracks at the stamping and flattening, and classify the stamping products. This method is a common test method in the field of step ladders.

[0099] Table 1 Mechanical properties test results

[0100] Tensile strength (MPa) Yield strength (MPa) Elongation (A50,%) Example 1 324 294 12.4 Example 2 320 290 12.8 Example 3 322 293 12.5 Example 4 316 287 12.2 Example 5 315 290 12.8 Example 6 318 294 12.5 Example 7 324 293 12.1 Example 8 358 327 12.4 Comparative Example 1 320 287 12.6 Comparative Example 2 319 281 13.1 Comparative Example 3 318 282 12.6 Comparative Example 4 319 287 12.7 Comparative Example 5 318 287 12.5 Comparative Example 6 320 289 12.6

[0101] By comparing the mechanical properties, we can find that:

[0102] Except for Example 8, which has a higher Cu content, a more obvious solid solution strengthening effect, and higher tensile strength and yield strength, the mechanical properties of other examples and comparative examples are not much different.

[0103] Table 2 Changes of Vickers hardness of extruded profiles with placement time

[0104]

[0105] By comparing the Webster hardness, we can find that:

[0106] In Example 1, within 7 days (168 hours) of natural aging, the Webster hardness is relatively low (≤5HW), and the hardness variation range is small. After 12 days of natural aging, the Webster hardness is 8HW, and the overall natural aging speed is slow. Under the same conditions, the hardness of Comparative Example 1 reaches 5HW after 12 hours of natural aging, 8HW after 2 days, and reaches the hardness peak of 11.5HW after 6 days.

[0107] In Example 2, within one day of natural aging, the Webster hardness is relatively low (≤5HW), and the hardness variation range is small. After 6 days of natural aging, the Webster hardness is 8HW, and the overall natural aging speed is slow. In the same case, in Comparative Example 2, the hardness reaches 5HW after 8 hours of natural aging, 8HW after 1 day, and reaches the hardness peak of 11.5HW after 7 days.

[0108] In Example 3, the Webster hardness is relatively low (≤5HW) within 12 hours of natural aging. After 3 days of natural aging, the Webster hardness is 8HW, and the overall natural aging speed is slow. In the same case, the hardness of Comparative Example 3 reaches 6HW after 6 hours of natural aging, 8HW after 8 hours, and reaches a hardness peak of 11.5HW after 20 hours.

[0109] In Example 4, the Webster hardness is relatively low (≤5HW) within 8 hours of natural aging, and the Webster hardness is 8HW after 1 day of natural aging. In the same case, the hardness of Comparative Example 4 reaches 6HW after 6 hours of natural aging, 8.5HW after 8 hours, and reaches the peak hardness of 11.5HW after 20 hours.

[0110] By analyzing Examples 1 to 4 and Comparative Examples 1 to 4, it can be found that the aluminum alloy of the present invention has a significant effect of delaying the natural aging process compared with the traditional 6061 alloy.

[0111] By analyzing Examples 3 and 5 and Comparative Examples 3, 5 and 6, it can be found that as the placement time after homogenization of the aluminum alloy of the present invention increases, the time for the Vickers hardness to increase to 5HW or 8HW gradually shortens, indicating that after the placement time after homogenization exceeds 30 days, the effect of Sn and In in inhibiting natural aging is weakened, but compared with the traditional 6061 alloy, it still has a more obvious inhibitory effect.

[0112] By analyzing Example 6 and Comparative Example 6, it can be found that after 100 days of homogenization, the cast rods are subjected to a short-term heating treatment and then extruded, which can partially restore the natural aging effect.

[0113] By analyzing Example 3 and Comparative Example 7, it can be found that as the amount of Sn+In added increases, the effect of inhibiting natural aging is improved.

[0114] By analyzing Example 3 and Example 8, it can be found that as the amount of Cu added increases, the strength gradually increases, and has a good effect of inhibiting natural aging.

[0115] Table 3 Stamping product grade classification

[0116] grade feature Typical image examples Level 1 No cracks at stamping See attached Figure 2 Level 2 There are non-penetrating micro cracks at the stamping See attached Figure 2 Level 3 There are obvious cracks at the stamping area, and the crack size is small See attached Figure 2 Level 4 There are obvious cracks at the stamping area, and the crack size is large See attached Figure 2 Level 5 The stamping part is completely cracked See attached Figure 2

[0117] Table 4 Storage time after flattening without cracking

[0118] Storage time (h) Example 1 285 Example 2 144 Example 3 50 Example 4 23 Example 5 43 Example 6 48 Example 7 66 Example 8 43 Comparative Example 1 47 Comparative Example 2 23 Comparative Example 3 8 Comparative Example 4 5 Comparative Example 5 25 Comparative Example 6 25

[0119] Table 5 Statistics of stamping product yield and stamping product grade

[0120]

[0121] Through the statistical comparison of the flattening experiment, we can find that:

[0122] In Example 1, within 7 days of natural aging, there was no cracking after flattening, the yield rate was 100%, and the stamping product grade was 1. When the storage time exceeded 285h, the grade of some stamping products was 3. Under the same conditions, the yield rate and stamping product grade of Comparative Example 1 decreased after 2 days of natural aging. On the 3rd day of natural aging, the yield rate was only 50%, and the stamping product grade was 1-4. On the 7th day of natural aging, all the stampings cracked, the product grade was 5, and the yield rate was 0%.

[0123] In Example 2, within 3 days of natural aging, there was no cracking after flattening, the yield rate was 100%, and the stamping product grade was 1. After 7 days of natural aging, some products had non-penetrating microcracks at the stamping, and the yield rate was 95%. Under the same conditions, in Comparative Example 2, within 24 hours of natural aging, some products had non-penetrating microcracks at the stamping, the yield rate was 99%, and the product grade was 1 to 2. After 48 hours of natural aging, all the stampings cracked, the product grade was 4 or 5, and the yield rate was 0%.

[0124] In Example 3, within 2 days of natural aging, there was no cracking after flattening, the yield rate was 100%, and the stamping product grade was 1. After 3 days of natural aging, some products had non-penetrating microcracks at the stamping, and a small number of products had obvious cracks of small size at the stamping, and the yield rate was 80%. After 7 days of natural aging, almost all the stamping products cracked, the product grade was 4 or 5, and the yield rate was 0%. In Comparative Example 3, there was no cracking after flattening within 8 hours of natural aging, and the stamping product grade was 1; with the extension of the natural aging time, the stamping product grade gradually increased. The yield rate of stamping products within 12 hours was 77%, and the stamping product grade was 1-4. After 1 day of natural aging, all stamping products cracked, the product grade was 4 or 5, and the yield rate was 0%.

[0125] Example 4: Within 12 hours of natural aging, there is no cracking after flattening, the yield rate is 100%, and the stamping product grade is 1. With the extension of natural aging time, some products have non-penetrating microcracks at the stamping parts. The yield rate of stamping products within 24 hours is 98%, and the stamping product grade is 1-2. After 2 days of natural aging, all stamping products are cracked, the product grade is 4 or 5, and the yield rate is 0%. Under the same conditions, comparative example 4 does not crack after flattening within 5 hours of natural aging, and the stamping product grade is 1; with the extension of natural aging time, the stamping product grade increases rapidly. The yield rate of stamping products within 12 hours is 58%, and the stamping product grade is 1-4. After 1 day of natural aging, all stamping products are cracked, the product grade is 4 or 5, and the yield rate is 0%.

[0126] By analyzing Examples 1 to 4 and Comparative Examples 1 to 4, it can be found that: within the range of 0-45°C, the effect of the Al-Mg-Si alloy produced by the present invention in inhibiting natural aging far exceeds that of the traditional 6061 alloy under the same placement conditions. And as the temperature decreases when the extruded profile is placed, the effect of the Al-Mg-Si alloy produced by the present invention in inhibiting natural aging gradually increases, and the time without cracking during stamping is significantly prolonged. When the profile is placed at 0-40°C, when the temperature is low, it will not crack even if it is placed for a long time (for example: 285h in Example 1) and flattened. As the placement temperature increases, the pinning effect of Sn and In on vacancies decreases rapidly, the effect of delaying natural aging is weakened, and the time without cracking during flattening is significantly shortened (for example: 23h in Example 4). However, compared with the traditional 6061 alloy, the time without cracking during flattening is extended by 4-5 times after adding Sn and In elements.

[0127] By analyzing Examples 3, 5 and Comparative Examples 5, 6, it can be found that the raw materials, implementation steps, homogenization treatment system, extrusion parameters, temperature during extrusion, online straightening parameters and aging treatment system selected during the melting and casting of the four cases are the same, and only the placement time after homogenization of the cast rods is significantly different. By counting the cracking time of each embodiment, it can be seen that the natural aging inhibition effect of the Al-Mg-Si alloy produced by the present invention gradually weakens with the extension of the placement time after homogenization. When the placement time after homogenization of the ingot exceeds 30 days, the extruded profile can only ensure that the natural aging will not crack during stamping within 25 hours. However, it can be seen from Example 6 that the cast rods placed for 100 days after homogenization are subjected to a short-term heating treatment and then extruded, and the time without cracking during stamping is extended to 48 hours. In traditional aluminum alloys, vacancies preferentially form vacancy pairs with MgSi clusters, resulting in a very fast natural aging process of aluminum alloys. After adding Sn and In elements, Sn and In capture a large number of supersaturated vacancies during the extrusion quenching cooling process, reducing the rapid precipitation process of MgSi clusters through vacancies, and delaying the process of natural aging. During the placement process after homogenization, MgSn phase gradually precipitates in the matrix, reducing the concentration of Sn atoms combined with vacancies during the natural aging process after extrusion. In the subsequent short-term heating treatment, MgSn phase re-dissolves, and Sn atoms continue to play a pinning role on vacancies, and the flattening time without cracking is extended again.

[0128] By analyzing Examples 3, 7, and 8, it can be found that with the increase in the amount of Sn+In added, the Al-Mg-Si alloy produced by the present invention further enhances the effect of inhibiting natural aging. However, the amount of Sn+In added should not exceed 0.12%. And with the increase in Cu content, while maintaining a good effect of delaying natural aging, the strength can be greatly improved.

[0129] In summary, the Al-Mg-Si aluminum alloy produced by the composition and process route designed by the present invention has a significant inhibitory effect on natural aging compared to the traditional 6061 alloy, can greatly extend the parking time of natural aging, is beneficial to the later deformation processing arrangement of aluminum alloy profiles, and improves production efficiency and yield rate.

[0130] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing an aluminum alloy material capable of delaying the natural aging process, characterized in that , including the following steps: S1: The ingredients are prepared according to the following mass percentages: Si 0.4-0.8%, Mg 0.8-1.2%, Fe≤0.15%, Cu 0.3-0.60%, Mn 0.04-0.08%, Cr 0.04-0.08%, Sn 0.04-0.08%, In≤ 0.04%, Zr 0.09-0.13%, Ti≤0.03%, Zn ≤0.02%, the balance is Al, a single impurity element is ≤0.05%, and the Mg / Si ratio is controlled between 1 and 2.4, wherein aluminum ingots are used, magnesium ingots are used, and master alloys are used for the remaining elements; the prepared raw materials are heated, melted, stirred, refined, slag-scraped, allowed to stand, degassed online, filtered, and cast to obtain aluminum alloy round ingots; S2: Perform multi-stage homogenization annealing on the aluminum alloy round ingot: heat up from room temperature to 420±5°C at a heating rate of 90°C / h, keep warm for 3-5 hours, then heat up to 530±5°C at a heating rate of 35°C / h, keep warm for 4-6 hours, then heat up to 570±5°C at a heating rate of 35°C / h, keep warm for 7-9 hours, then quickly cool to room temperature to obtain a homogenized aluminum alloy round bar A, which is then placed; S3: When the placement time of the aluminum alloy round bar A in S2 is greater than 30 days, short-term heating is performed, the temperature is raised from room temperature to 560±5°C at a heating rate of 90°C / h, and the temperature is kept for 2 hours, and then the aluminum alloy round bar B is obtained by rapid cooling; when the placement time of the aluminum alloy round bar A is less than or equal to 30 days, the step S4 is directly performed; S4: heating and extruding the aluminum alloy round bar A or B to obtain a profile, and performing online quenching on the extruded profile. The online quenching adopts strong wind cooling quenching, and the cooling rate of the profile in the temperature range from extrusion to cooling to 200° C. is 12-15° C. / s; S5: After the profile is cooled down to room temperature online, it is straightened and flattened: when the room temperature is 5±5℃, the straightened profile is flattened within 285h; when the room temperature is 15±5℃, the straightened profile is flattened within 144h; when the room temperature is 25±5℃, the straightened profile is flattened within 50h; when the room temperature is 35±5℃, the straightened profile is flattened within 23h; S6: The flattened profile of S5 is aged in an aging furnace at a temperature of 180±3℃ and a holding time of 4h.

2. The method for preparing the aluminum alloy material according to claim 1, characterized in that: In the above-mentioned S1, the temperature of heating and melting is 700-800°C.

3. The method for preparing the aluminum alloy material according to claim 1, characterized in that: In S1, the aluminum alloy melt obtained after standing is transferred to a flow channel. During the flow channel transfer, a grain refiner is added to the flow channel, and then online degassing and filtering are performed.

4. The method for preparing the aluminum alloy material according to claim 3, characterized in that: The grain refiner is an aluminum-titanium-boron grain refiner.

5. The method for preparing the aluminum alloy material according to claim 1, characterized in that: In the above S4, the heating temperature is 450-550°C.

6. The method for preparing the aluminum alloy material according to claim 1, characterized in that: In S4, the extrusion speed is 3.6-4.5 mm / s, and the outlet temperature of the front beam of the extrusion is ≥525°C.

7. The method for preparing the aluminum alloy material according to claim 1, characterized in that: In S5, the straightness of the profile after straightening is ≤0.5 mm / m.