A method for smelting clean steel, and clean steel

Through the clean steel smelting method combining arc furnace smelting, LF refining and RH refining, the problems of high impurity elements and high nitrogen content in arc furnace steel are solved, and low carbon emissions and high cleanliness production of automotive steel is achieved, which meets the needs of the Quality requirements for automotive steel.

CN118272719BActive Publication Date: 2024-11-19BEIJING SHOUGANG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410522302.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-11-19
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

On the basis of meeting low carbon emissions, it is difficult for the existing technology to improve the cleanliness of automotive steel, especially because the content of Cu, Sn, Cr and other impurities in arc furnace steel is high and the nitrogen content is high, resulting in the thermal ductility of the steel. Reduction and internal crack problems cannot meet the quality requirements of automotive steel.

Method used

A clean steel smelting method is adopted, including smelting scrap steel, deoxygenation and slag eluting, LF refining deep desulfurization, RH refining oxygen blown decarbonization and vacuum denitrogenation, and finally obtaining clean steel through full protection casting, controlling the steel The nitrogen, carbon and sulfur content in water is below 0.003%.

Benefits of technology

It minimizes carbon dioxide emissions, significantly reduces nitrogen content, improves the cleanliness of automotive steel, meets the quality requirements of automotive steel, and reduces the thermal ductility problems and internal crack risks of steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118272719B_ABST
    Figure CN118272719B_ABST
Patent Text Reader

Abstract

The present invention provides a smelting method of clean steel and clean steel, which belongs to the field of steel preparation. The method comprises: smelting scrap steel to obtain a first molten steel; performing steel-tapping deoxidation and slag-washing desulfurization on the first molten steel to obtain a second molten steel; performing deep desulfurization and heating on the second molten steel through LF refining to obtain a first refined molten steel; performing oxygen blowing decarburization and vacuum denitrification on the first refined molten steel through RH refining to obtain a second refined molten steel; performing full-protection pouring on the second refined molten steel to obtain clean steel. By using an electric furnace to melt recycled scrap steel that can be regarded as having near-zero carbon emissions, carbon dioxide emissions are minimized, and at the same time, coupled with LF refining and RH refining, the nitrogen content is minimized. Thereby, the production of high-quality, low-nitrogen automotive steel with low carbon emissions is achieved through a short process of an electric furnace.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of steel preparation technology, and in particular to a method for smelting clean steel and clean steel. Background Art

[0002] Against the backdrop of dual carbon emissions both domestically and internationally, automakers, especially those in Europe, have put forward requirements for reducing carbon emissions in automotive steel and have made it an important criterion for selecting suppliers in the future.

[0003] In recent years, the importance of electric arc furnace steelmaking has been reiterated both domestically and internationally from the perspectives of energy conservation and resource recycling. For various reasons, the output of steel produced using electric arc furnaces has been increasing. However, in terms of steel quality, electric arc furnace steel contains higher levels of impurity elements such as Cu, Sn, and Cr than converter steel, and the nitrogen content is particularly high. High nitrogen content reduces the hot ductility of the steel, leading to, for example, the brittleness of aluminum nitride and the development of internal and surface cracks in the casting chips during continuous casting, which do not meet the quality requirements for automotive steel. Therefore, in the production process of automotive steel, improving the cleanliness of automotive steel while meeting low carbon emissions is a technical issue that urgently needs to be addressed. Summary of the Invention

[0004] This application provides a method for smelting clean steel and clean steel, in order to solve the technical problem in the prior art that it is difficult to improve the cleanliness of automotive steel while meeting the requirements of low carbon emissions.

[0005] In a first aspect, this application provides a method for smelting clean steel, the method comprising:

[0006] The scrap steel is melted down to obtain the first molten steel;

[0007] The first molten steel is subjected to deoxidation and slag washing desulfurization to obtain the second molten steel;

[0008] The second molten steel is subjected to deep desulfurization and heated by LF refining to obtain the first refined molten steel;

[0009] The first refined molten steel is subjected to oxygen blowing for decarburization and vacuum denitrification through RH refining to obtain the second refined molten steel;

[0010] The second refined molten steel is poured under full protection to obtain clean steel.

[0011] Optionally, in the first molten steel, the mass fraction of carbon is 0.03% to 0.04%, the mass fraction of oxygen is 0.050% to 0.080%, the mass fraction of nitrogen is 0.005% to 0.007%, and the mass fraction of sulfur is 0.007% to 0.014%.

[0012] Optionally, the temperature of the first molten steel is 1590℃~1620℃.

[0013] Optionally, the raw materials added for steel tapping deoxidation include: 0.50 kg / t steel to 1 kg / t steel deoxidizer, and the raw materials added for slag washing desulfurization include: 5 kg / t steel to 10 kg / t steel activated quicklime and 2 kg / t steel to 4 kg / t steel slag deoxidizer.

[0014] Optionally, in the first refined molten steel, the mass fraction of sulfur is ≤0.001%, and the mass fraction of carbon is 0.03% to 0.04%; the temperature of the first refined molten steel is 1640℃ to 1660℃.

[0015] Optionally, the raw materials added for the deep desulfurization include: 20 kg / t·steel to 30 kg / t·steel of activated quicklime and 2 kg / t·steel to 4 kg / t·steel of bauxite.

[0016] Optionally, during the deep desulfurization process, a carrier gas is used for bottom blowing and stirring, and the flow rate of the carrier gas is 800 NL / min to 1200 NL / min.

[0017] Optionally, the step of subjecting the first refined molten steel to oxygen blowing decarburization and vacuum denitrification through RH refining to obtain the second refined molten steel includes:

[0018] The first refined molten steel is transferred to an RH refining furnace, where it is subjected to oxygen blowing and pure decarburization under deep vacuum conditions to obtain decarburized molten steel with a set carbon mass fraction; the pure decarburization treatment time after oxygen blowing is ≥15 min, and the set carbon mass fraction is ≤0.0025%.

[0019] The decarburized molten steel is subjected to deoxidation and alloying treatment, followed by deep vacuum treatment to obtain the second refined molten steel; the deep vacuum treatment time is ≥15min and the vacuum degree is ≤0.10KPa.

[0020] Optionally, the oxygen blowing rate in the oxygen blowing operation satisfies the following relationship: Q ≥ [C] / 0.0001%,

[0021] In the formula, Q represents the oxygen blowing volume in the oxygen blowing operation, with units of Nm³. 3 [C] represents the mass fraction of carbon in the first refined molten steel.

[0022] Secondly, this application provides a clean steel prepared by the method described in any one of the embodiments of the first aspect, wherein the mass fraction of nitrogen is ≤0.003%, the mass fraction of carbon is ≤0.003%, and the mass fraction of sulfur is ≤0.003%.

[0023] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0024] This application provides a method for smelting clean steel. By using an electric furnace to melt recycled scrap steel that can be considered as having near-zero carbon emissions, carbon dioxide emissions are minimized. Simultaneously, it is coupled with LF refining and RH refining to minimize nitrogen content. Furthermore, the use of deep LF desulfurization creates favorable conditions for RH vacuum denitrification. This solves the technical problem in existing technologies of the difficulty in improving the cleanliness of automotive steel while meeting low carbon emission requirements. Attached Figure Description

[0025] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0026] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.

[0027] Figure 1 This is a schematic flowchart of a clean steel smelting method provided in an embodiment of this application. DETAILED DESCRIPTION

[0028] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0029] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.

[0030] Furthermore, in the description of this application, the terms "comprising," "including," etc., mean "including but not limited to." In this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this document, "and / or" describes the relationship between related objects, indicating that three relationships can exist; for example, A and / or B can represent: A alone, A and B simultaneously, or B alone. A and B can be singular or plural. In this document, "at least one" means one or more, and "more than" means two or more. "At least one," "at least one of the following," or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple.

[0031] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0032] Figure 1 This is a schematic flowchart of a clean steel smelting method provided in an embodiment of this application.

[0033] See Figure 1 This application provides a method for smelting clean steel, the method comprising:

[0034] S1. Smelt the scrap steel to obtain the first molten steel;

[0035] In some embodiments, the mass fraction of carbon in the first molten steel is 0.03% to 0.04%, the mass fraction of oxygen is 0.050% to 0.080%, the mass fraction of nitrogen is 0.005% to 0.007%, and the mass fraction of sulfur is 0.007% to 0.014%. It should be noted that if the mass fraction of carbon in the molten steel is too low, it will result in high oxygen content and high deoxidizer consumption; if the mass fraction of carbon in the molten steel is too high, additional carbon will be required in the electric furnace, affecting the efficiency of the electric furnace. The mass fraction of carbon in the molten steel can be 0.03% to 0.04%, which can reduce the final oxygen content and reduce the consumption of deoxidizers for tapping. The mass fraction of oxygen in the molten steel can be 0.050% to 0.080%, and the oxygen content is determined by the carbon content based on the stirring capacity of the electric furnace. The mass fraction of nitrogen in molten steel is 0.005% to 0.007%, and the mass fraction of sulfur is 0.007% to 0.014%. Nitrogen is a harmful element that requires strict control in this application. Nitrogen control is difficult in electric furnace processes using all scrap steel as raw material, so the nitrogen content is minimized. The mass fraction of sulfur in molten steel is 0.007% to 0.014%. Excessive sulfur content results in a large amount of desulfurization in the process, resulting in a longer cycle time and affecting the matching of process cycles. Excessive sulfur content requires reducing the addition of low-cost, high-sulfur scrap steel, which increases costs. For example, the mass fraction of carbon in the molten steel can be 0.03%, 0.035%, 0.04%, etc.; the mass fraction of oxygen in the molten steel can be 0.050%, 0.055%, 0.060%, 0.070%, 0.080%, etc.; the mass fraction of nitrogen in the molten steel can be 0.005%, 0.006%, 0.007%, etc.; and the mass fraction of sulfur can be 0.007%, 0.008%, 0.009%, 0.010%, 0.012%, 0.013%, 0.014%, etc.

[0036] In some embodiments, the temperature of the first molten steel is 1590°C to 1620°C. It should be noted that, considering the subsequent LF furnace heating cycle, a tapping temperature of the molten steel above this range causes unnecessary waste, while a tapping temperature below this range increases the LF heating cycle, resulting in a mismatch between process cycles, thereby affecting overall production efficiency. For example, the temperature of the molten steel can be 1590°C, 1595°C, 1600°C, 1605°C, 1610°C, 1615°C, 1620°C, etc.

[0037] S2, performing tapping deoxidation and slag washing desulfurization on the first molten steel to obtain a second molten steel;

[0038] In some embodiments, the raw materials added for steel tapping deoxidation include: 0.50 kg / t·steel to 1 kg / t·steel deoxidizer, and the raw materials added for slag washing desulfurization include: 5 kg / t·steel to 10 kg / t·steel activated quicklime and 2 kg / t·steel to 4 kg / t·steel slag deoxidizer. It should be noted that the amount of raw materials added for steel tapping deoxidation can be calculated based on the actual oxygen content of the tapped steel, at a rate of 0.1 kg / t·steel to 0.125 kg / t·steel for 0.01% oxygen. The raw materials for slag washing desulfurization can be quicklime and slag deoxidizer added based on the oxygen content and slag oxidizing properties. For 0.01% oxygen, 1 kg / t·steel to 1.25 kg / t·steel quicklime and 0.4 kg / t·steel to 0.5 kg / t·steel slag deoxidizer are added. Adding too much increases costs and causes waste, while adding too little will not achieve the desired slag washing desulfurization effect. For example, the amount of deoxidizer added is 0.50 kg / t·steel, 0.60 kg / t·steel, 0.70 kg / t·steel, 0.80 kg / t·steel, 1 kg / t·steel, etc., the amount of activated quicklime added is 5 kg / t·steel, 6 kg / t·steel, 7 kg / t·steel, 8 kg / t·steel, 9 kg / t·steel, 10 kg / t·steel, etc., and the amount of slag deoxidizer added can be 2 kg / t·steel, 2.5 kg / t·steel, 3 kg / t·steel, 3.5 kg / t·steel, 4 kg / t·steel, etc.

[0039] S3. The second molten steel is subjected to deep desulfurization and heated by LF refining to obtain the first refined molten steel;

[0040] Oxygen and sulfur active atoms have a significant impact on the RH vacuum denitrification rate. The LF deep desulfurization method is adopted to create favorable conditions for subsequent RH vacuum denitrification.

[0041] In some embodiments, the mass fraction of sulfur in the first refined molten steel is ≤0.001%, and the mass fraction of carbon is 0.03% to 0.04%; the temperature of the first refined molten steel is 1640℃ to 1660℃. It should be noted that a sulfur mass fraction ≤0.001% is necessary to achieve the desired denitrification effect. A carbon mass fraction of 0.03% to 0.04% avoids excessive RH oxygen blowing, which could prolong the cycle, while maintaining oxygen control in the electric furnace. The temperature of the first refined molten steel, 1640℃ to 1660℃, can be matched with the RH refining cycle and temperature drop, ultimately ensuring that the casting is within a suitable superheat range. For example, the mass fraction of sulfur in the first refined molten steel can be 0.0005%, 0.0006%, 0.0007%, 0.0008%, 0.0009%, 0.0010%, etc.; the temperature of the first refined molten steel can be 1640℃, 1645℃, 1650℃, 1655℃, 1660℃, etc.

[0042] In some embodiments, the raw materials added for deep desulfurization include: 20 kg / t·steel to 30 kg / t·steel of activated quicklime and 2 kg / t·steel to 4 kg / t·steel of bauxite. It should be noted that the quicklime and slag deoxidizer are added according to the oxygen content and slag oxidizing properties. Adding too much increases costs and causes waste, while adding too little will not achieve the expected desulfurization effect. For example, the amount of activated quicklime added is 20 kg / t·steel, 22 kg / t·steel, 24 kg / t·steel, 26 kg / t·steel, 28 kg / t·steel, 30 kg / t·steel, etc., and the amount of bauxite added is 2 kg / t·steel, 2.5 kg / t·steel, 3 kg / t·steel, 3.5 kg / t·steel, 4 kg / t·steel, etc.

[0043] In some embodiments, during the deep desulfurization process, a carrier gas is used for bottom blowing and stirring, with a flow rate of 800 NL / min to 1200 NL / min. It should be noted that if the carrier gas flow rate is too high, it will cause splashing of molten steel, resulting in metal loss; if the flow rate is too low, it will affect the desulfurization effect. A carrier gas flow rate of 800 NL / min to 1200 NL / min can fully mix the desulfurization raw materials with the molten steel, thereby ensuring the desulfurization effect. For example, the carrier gas flow rate can be 800 NL / min, 900 NL / min, 1000 NL / min, 1100 NL / min, 1200 NL / min, etc.

[0044] S4, performing oxygen decarburization and vacuum denitrification on the first refined molten steel by RH refining to obtain a second refined molten steel;

[0045] In some embodiments, the step of subjecting the first refined molten steel to oxygen blowing decarburization and vacuum denitrification via RH refining to obtain the second refined molten steel includes:

[0046] The first refined molten steel is transferred to an RH refining furnace, and oxygen blowing and pure decarburization are performed under vacuum conditions to obtain decarburized molten steel, wherein the mass fraction of carbon in the decarburized molten steel is ≤0.0025%;

[0047] The decarburized molten steel undergoes deoxidation and alloying treatment, followed by deep vacuum treatment to obtain the second refined molten steel; the deep vacuum treatment time is ≥15 minutes. It should be noted that maintaining deep vacuum treatment for ≥15 minutes after deoxidation and alloying ensures that inclusions are fully floated and removed, thereby guaranteeing that the cleanliness of the molten steel meets the requirements of the steel grade. For example, the deep vacuum treatment time can be 15 minutes, 16 minutes, 17 minutes, 18 minutes, 19 minutes, 20 minutes, etc.

[0048] In some embodiments, the time of the pure decarburization treatment after oxygen blowing is ≥15 min, and the oxygen blowing amount of the oxygen blowing operation satisfies the following relationship: Q ≥ [C] / 0.0001%,

[0049] In the formula, Q represents the oxygen blowing volume in the oxygen blowing operation, with units of Nm³. 3 ; [C] represents the mass fraction of carbon in the first refined molten steel.

[0050] It should be noted that, under the aforementioned oxygen blowing amount, a pure decarburization treatment time of ≥15 minutes under deep vacuum conditions can ensure that the carbon content is stably reduced to below 25 ppm. The oxygen blowing amount during the oxygen blowing operation satisfies the following relationship: Q ≥ [C] / 0.0001%, which ensures that the desired decarburization effect is achieved. Otherwise, the decarburization rate will be slow, affecting efficiency. By controlling the oxygen blowing amount and decarburization time, the mass fraction of carbon in the molten steel can be guaranteed to be ≤0.0025%. For example, the pure decarburization treatment time can be 15 minutes, 16 minutes, 17 minutes, 18 minutes, 19 minutes, 20 minutes, etc.

[0051] S5. The second refined molten steel is poured under full protection to obtain clean steel.

[0052] Based on a general inventive concept, the present application provides a clean steel, in which the mass fraction of nitrogen is ≤0.003%, the mass fraction of carbon is ≤0.003%, and the mass fraction of sulfur is ≤0.003%.

[0053] The clean steel is achieved based on the above-mentioned method for preparing clean steel. The specific steps of the method for preparing clean steel can be referred to the above-mentioned embodiment. Since the clean steel adopts part or all of the technical solutions of the above-mentioned embodiment, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be repeated here.

[0054] The present application will be further described below in conjunction with specific examples. It should be understood that these examples are intended to illustrate the present application only and are not intended to limit the scope of the present application. The experimental methods in the following examples where specific conditions are not specified are generally measured according to industry standards. If there are no corresponding industry standards, then the methods are carried out according to general international standards, conventional conditions, or the conditions recommended by the manufacturer.

[0055] Example 1

[0056] Example 1 provides a method for smelting clean steel. This method adopts the process route of electric arc furnace → electric arc furnace tapping deoxidation and desulfurization → LF → RH → continuous casting. The smelting process is as follows:

[0057] S11. High-quality scrap steel is added to an electric arc furnace and melted by electricity. During the process, argon gas is introduced into the bottom of the furnace for stirring. Carbon powder and oxygen are injected into the top of the molten pool through an oxygen lance to create foamy slag. Carbon blocks are added into the molten pool to obtain the first molten steel. The final temperature of the molten steel is 1595℃. The mass fraction of carbon in the molten steel is 0.0382%, the mass fraction of oxygen is 0.0651%, the mass fraction of nitrogen is 0.0053%, and the mass fraction of sulfur is 0.013%.

[0058] S21. The first molten steel is deoxidized during tapping and then washed with lime and slag deoxidizer for desulfurization. Based on the mass of 1 ton of molten steel, the amount of deoxidizer added is 0.66 kg, the amount of lime added is 6.63 kg, and the amount of slag deoxidizer added is 2.73 kg, to obtain the second molten steel.

[0059] S31. The second ladle of molten steel is transferred to the ladle refining furnace for further desulfurization and heating. Based on the mass of 1 t of the second molten steel, the amount of quicklime added is 28.9 kg, the amount of bauxite added is 3.8 kg, and the oxygen blowing rate for bottom blowing is 800 NL / min. The first refined molten steel is obtained. The temperature of the first refined molten steel is 1642℃. The mass fraction of sulfur in the first refined molten steel is 0.0009%, and the mass fraction of carbon is 0.0372%.

[0060] S41. The first refined steel is subjected to oxygen blowing decarburization under RH ultimate vacuum, with an RH oxygen blowing rate of 375 Nm³. 3 After oxygen blowing, pure decarburization was carried out for 15.8 minutes. After deoxidation and alloying, deep vacuum was maintained for 16.3 minutes to obtain the second refined molten steel. The mass fraction of nitrogen in the second refined molten steel was 0.0027%, the mass fraction of carbon was 0.0023%, and the mass fraction of sulfur was 0.0030%.

[0061] S51. The second refined molten steel is poured under full protection to prevent nitrogen from increasing in the molten steel, resulting in clean steel with a nitrogen mass fraction of 0.0028%, a carbon mass fraction of 0.0024%, and a sulfur mass fraction of 0.0030%.

[0062] Example 2

[0063] Example 2 provides a method for smelting clean steel. This method adopts the process route of electric arc furnace → electric arc furnace tapping deoxidation and desulfurization → LF → RH → continuous casting. The smelting process is as follows:

[0064] S11. High-quality scrap steel is added to an electric arc furnace and melted by electricity. During the process, argon gas is introduced into the bottom of the furnace for stirring. Carbon powder and oxygen are injected into the top of the molten pool through an oxygen lance to create foamy slag. Carbon blocks are added into the molten pool to obtain the first molten steel. The final temperature of the molten steel is 1591℃. The mass fraction of carbon in the molten steel is 0.0310%, the mass fraction of oxygen is 0.0758%, the mass fraction of nitrogen is 0.0065%, and the mass fraction of sulfur is 0.011%.

[0065] S21. The first molten steel is deoxidized during tapping and then washed with lime and slag deoxidizer for desulfurization. Based on the mass of 1 ton of molten steel, the amount of deoxidizer added is 0.78 kg, the amount of lime added is 7.66 kg, and the amount of slag deoxidizer added is 3.7 kg, to obtain the second molten steel.

[0066] S31. The second ladle of molten steel is transferred to the ladle refining furnace for further desulfurization and heating. Based on the mass of 1 t of the second molten steel, the amount of quicklime added is 25.8 kg, the amount of bauxite added is 3.1 kg, and the oxygen blowing rate for bottom blowing is 900 NL / min. The first refined molten steel is obtained. The temperature of the first refined molten steel is 1652℃. The mass fraction of sulfur in the first refined molten steel is 0.0007%, and the mass fraction of carbon is 0.0328%.

[0067] S41, the first refined molten steel is subjected to oxygen blowing decarburization under RH extreme vacuum, with the RH oxygen blowing amount being 350Nm 3 After oxygen blowing, pure decarburization was carried out for 15.3 minutes. After deoxidation and alloying, deep vacuum was maintained for 18.3 minutes to obtain the second refined molten steel. The mass fraction of nitrogen in the second refined molten steel was 0.0028%, the mass fraction of carbon was 0.0018%, and the mass fraction of sulfur was 0.0027%.

[0068] S51. The second refined molten steel is poured under full protection to prevent nitrogen from increasing in the molten steel, resulting in clean steel with a nitrogen mass fraction of 0.0028%, a carbon mass fraction of 0.0020%, and a sulfur mass fraction of 0.0026%.

[0069] Example 3

[0070] Example 3 provides a clean steel smelting method, which adopts a process route of electric arc furnace → electric furnace steel tapping deoxidation and desulfurization → LF → RH → continuous casting, and adopts the following smelting process, specifically:

[0071] S11. High-quality scrap steel is added to an electric arc furnace and melted by electricity. During the process, argon gas is introduced into the bottom of the furnace for stirring. Carbon powder and oxygen are injected into the top of the molten pool through an oxygen lance to create foamy slag. Carbon blocks are added into the molten pool to obtain the first molten steel. The final temperature of the molten steel is 1606℃. The mass fraction of carbon in the molten steel is 0.0323%, the mass fraction of oxygen is 0.0709%, the mass fraction of nitrogen is 0.0051%, and the mass fraction of sulfur is 0.008%.

[0072] S21. The first molten steel is deoxidized during tapping and then washed with quicklime and slag deoxidizer for desulfurization. Based on the mass of 1 ton of molten steel, the amount of deoxidizer added is 0.85 kg, the amount of quicklime added is 7.3 kg, and the amount of slag deoxidizer added is 3.4 kg, to obtain the second molten steel.

[0073] S31. The second ladle of molten steel is transferred to the ladle refining furnace for further desulfurization and heating. Based on the mass of 1 t of the second molten steel, the amount of quicklime added is 21.2 kg, the amount of bauxite added is 2.3 kg, and the oxygen blowing rate for bottom blowing is 1200 NL / min. The first refined molten steel is obtained. The temperature of the first refined molten steel is 1656℃. The mass fraction of sulfur in the first refined molten steel is 0.0005%, and the mass fraction of carbon is 0.0318%.

[0074] S41. The first refined steel is subjected to oxygen blowing decarburization under RH ultimate vacuum, with an RH oxygen blowing rate of 330 Nm³. 3 After oxygen blowing, pure decarburization was carried out for 16.8 minutes. After deoxidation and alloying, deep vacuum was maintained for 19.2 minutes to obtain the second refined molten steel. The mass fraction of nitrogen in the second refined molten steel was 0.0025%, the mass fraction of carbon was 0.0015%, and the mass fraction of sulfur was 0.0021%.

[0075] S51. The second refined molten steel is poured under full protection to prevent nitrogen from increasing in the molten steel, resulting in clean steel with a nitrogen mass fraction of 0.0026%, a carbon mass fraction of 0.0018%, and a sulfur mass fraction of 0.0022%.

[0076] Comparative Example 1

[0077] Comparative Example 1 provides a method for smelting high-strength steel. This method adopts an electric arc furnace → RH → continuous casting process, and the smelting process is as follows:

[0078] S11. High-quality scrap steel is added to an electric arc furnace and melted by electricity. During the process, argon gas is introduced into the bottom of the furnace for stirring. Carbon powder and oxygen are injected into the top of the molten pool through an oxygen lance to create foamy slag, thus obtaining molten steel. The final temperature of the molten steel is controlled at 1664℃, the final carbon mass fraction is 0.059%, the final oxygen mass fraction is 0.0824%, and the final nitrogen mass fraction is 0.0063%.

[0079] S21. Molten steel is subjected to a natural decarburization process under RH ultimate vacuum, with a pure circulation time of 4 minutes, to obtain refined molten steel. The mass fraction of nitrogen in the refined molten steel is 0.0045%, the mass fraction of carbon is 0.0014%, and the mass fraction of sulfur is 0.0075%. The refined molten steel is then subjected to full protective casting to prevent nitrogen accumulation, resulting in steel with a nitrogen mass fraction of 0.0048%.

[0080] Comparative Example 2

[0081] Comparative Example 2 provides a method for smelting high-strength steel. This method adopts an electric arc furnace → RH → continuous casting process, and the smelting process is as follows:

[0082] S11. High-quality scrap steel is added to an electric arc furnace and melted by electricity. During the process, argon gas is introduced into the bottom of the furnace for stirring. Carbon powder and oxygen are injected into the top of the molten pool through an oxygen lance to create foamy slag, thus obtaining the first molten steel. The final temperature of the molten steel is controlled at 1675℃, the final carbon mass fraction is 0.076%, the final oxygen mass fraction is 0.0675%, and the final nitrogen mass fraction is 0.0072%.

[0083] S21. Under RH ultimate vacuum, a natural decarburization process is adopted, ensuring a pure circulation time of 4.5 minutes, to obtain refined molten steel with a nitrogen mass fraction of 0.0050%, a carbon mass fraction of 0.0025%, and a sulfur mass fraction of 0.0059%. The refined molten steel is then subjected to full protective casting to prevent nitrogen accumulation, resulting in steel with a nitrogen mass fraction of 0.0052%.

[0084] Comparative Example 3

[0085] Comparative Example 3 provides a method for smelting high-strength steel. This method adopts an electric arc furnace → RH → continuous casting process, and the smelting process is as follows:

[0086] S11. High-quality scrap steel is added to an electric arc furnace and melted by electricity. During the process, argon gas is introduced into the bottom of the furnace for stirring. Carbon powder and oxygen are injected into the top of the molten pool through an oxygen lance to create foamy slag, thus obtaining the first molten steel. The final temperature of the molten steel is controlled at 1658℃, the final carbon mass fraction is 0.065%, the final oxygen mass fraction is 0.0732%, and the final nitrogen mass fraction is 0.0078%.

[0087] S21. Under RH ultimate vacuum, a natural decarburization process is adopted, ensuring a pure circulation time of 4.2 minutes, to obtain refined molten steel with a nitrogen mass fraction of 0.0053%, a carbon mass fraction of 0.0019%, and a sulfur mass fraction of 0.0082%. The refined molten steel is then subjected to full protective casting to prevent nitrogen accumulation, resulting in steel with a nitrogen mass fraction of 0.0053%.

[0088] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A method for smelting clean steel, characterized in that: The method comprises: Melting the scrap steel to obtain first molten steel; The first molten steel is subjected to steel-tapping deoxidation and slag-washing desulfurization to obtain a second molten steel; The second molten steel is subjected to deep desulfurization and temperature increase through LF refining to obtain a first refined molten steel; The first refined molten steel is subjected to oxygen blowing decarburization and vacuum denitrification by RH refining to obtain a second refined molten steel; The second refined molten steel is fully poured to obtain clean steel; In the first molten steel, the mass fraction of carbon is 0.03% to 0.04%, the mass fraction of oxygen is 0.050% to 0.080%, the mass fraction of nitrogen is 0.005% to 0.007%, and the mass fraction of sulfur is 0.007% to 0.014%; The raw materials added for steel tapping deoxidation include: 0.50Kg / t·steel to 1Kg / t·steel deoxidizer, and the raw materials added for slag washing desulfurization include: 5Kg / t·steel to 10Kg / t·steel active lime and 2Kg / t·steel to 4Kg / t·steel slag deoxidizer; In the first refined molten steel, the mass fraction of sulfur is ≤0.001%; The raw materials added for deep desulfurization include: 20Kg / t·steel to 30Kg / t·steel active lime, 2Kg / t·steel to 4Kg / t·steel bauxite; In the deep desulfurization process, a carrier gas is used for bottom blowing and stirring, and the flow rate of the carrier gas is 800NL / min~1200NL / min; The method of subjecting the first refined molten steel to oxygen decarburization and vacuum denitrification through RH refining to obtain a second refined molten steel comprises: The first refined molten steel is transferred to an RH refining furnace, and oxygen blowing and pure decarburization are performed under deep vacuum conditions to obtain decarburized molten steel with a set carbon mass fraction; the time of the pure decarburization treatment after oxygen blowing is ≥15 minutes, and the set carbon mass fraction is ≤0.0025%; The decarburized molten steel is subjected to deoxidation and alloying treatment, and then subjected to deep vacuum treatment to obtain a second refined molten steel; the deep vacuum treatment time is ≥15 min, and the vacuum degree is ≤0.10 KPa; In the clean steel, the mass fraction of nitrogen is ≤0.003%, the mass fraction of carbon is ≤0.003%, and the mass fraction of sulfur is ≤0.003%.

2. The method according to claim 1, characterized in that The temperature of the first molten steel is 1590°C to 1620°C.

3. The method according to claim 1, characterized in that In the first refined molten steel, the mass fraction of carbon is 0.03%-0.04%; the temperature of the first refined molten steel is 1640°C-1660°C.

4. The method according to claim 1, characterized in that: The oxygen blowing amount of the oxygen blowing operation satisfies the following relationship: Q ≥ [C] / 0.0001%, Wherein, Q represents the oxygen blowing amount value of the oxygen blowing operation, the unit is Nm 3 ; [C] represents the mass fraction of carbon in the first refined molten steel.