High-strength aluminum-magnesium alloy pre-nickel-plated strip and its production process

Through the synergistic effect of forming a dense nano-coating and a stress regulator on the surface of the aluminum-magnesium alloy, the problem of poor bonding between the aluminum-magnesium alloy and the nickel coating is solved, and the corrosion resistance and mechanical properties of the nickel coating are significantly improved.

CN118272877BActive Publication Date: 2024-10-15SHENZHEN YUKUANG NEW MATERIALS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410405812.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-07
Publication Date
2024-10-15
Estimated Expiration
2044-04-07

AI Technical Summary

Technical Problem

The poor bonding between aluminum-magnesium alloy and nickel plating results in poor corrosion resistance and wear resistance, and the high porosity of the nickel plating layer affects the processing performance and mechanical properties.

Method used

A pre-plated nickel layer is formed on the surface of the aluminum-magnesium alloy through electroplating nickel solution, and SiO2 particles of different particle sizes are added for modification to form a dense nano-plating layer, and polylactic acid, sodium o-benzoylsulfonimide and saccharin are used as stress adjustment The agent eliminates the internal stress of the nickel plating layer and improves the bonding force between the nickel plating layer and the base material.

Benefits of technology

It significantly improves the corrosion resistance, hardness, tensile strength, yield strength and elongation of the nickel plating layer, improves the fine uniformity and bonding strength of the nickel plating layer, and enhances the overall performance of the aluminum-magnesium alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004777266600000071
    Figure BDA0004777266600000071
  • Figure BDA0004777266600000081
    Figure BDA0004777266600000081
Patent Text Reader

Abstract

The present invention provides a high-strength aluminum-magnesium alloy pre-nickel-plated strip and a production process thereof. A pre-nickel-plated layer is formed on the surface of the aluminum-magnesium alloy by electroplating nickel solution, and two SiO2 with different particle sizes are added to the electroplating nickel solution. 2 The particles are coupled to form a dense nano-coating, and different modifiers are used to modify the two SiO 2 The particles are fully dispersed and evenly coupled to form a denser nano-plating layer, and the synergistic enhancement of micro-nano particles is exerted, which significantly improves the corrosion resistance, hardness, tensile strength, yield strength and elongation of the nano-nickel plating layer. In addition, three stress regulators, polylactic acid, sodium o-benzoylsulfonyl imide and saccharin, are added at the same time to synergistically eliminate the internal stress of the nickel plating layer, improve the bonding strength between the nickel plating layer and the substrate, make the nickel plating layer more delicate and uniform, and thus show better corrosion resistance, tensile strength, yield strength and elongation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of aluminum-magnesium alloy strips, and in particular relates to an aluminum-magnesium alloy pre-nickel-plated strip and a production process thereof. Background Art

[0002] Aluminum and magnesium are abundant and inexpensive, and aluminum-magnesium alloys have good plasticity and processability, are not easily corroded, and have a long service life. They are widely used in aerospace and defense, communications electronics, medical equipment, household appliances, and especially new energy vehicles. However, their poor corrosion resistance and wear resistance limit the application of aluminum-magnesium alloys. Nickel has a strong passivation ability and can form a passivation film on the surface of the substrate, and is therefore widely used to improve the corrosion resistance of aluminum-magnesium alloy surfaces. However, aluminum-magnesium alloys have poor adhesion to nickel coatings, which easily leads to blistering and delamination, resulting in poor corrosion resistance and wear resistance. On the other hand, the nickel coating has a high porosity, and the coating thickness usually needs to be increased to more than 25 microns to achieve a pore-free effect. The increase in coating thickness further makes it prone to delamination and affects the processing properties, tensile strength, elongation, and other properties of the aluminum-magnesium alloy. Therefore, how to provide an aluminum-magnesium alloy pre-nickel-plated strip with a thin nickel coating that simultaneously has corrosion resistance, tensile strength, elongation, and processing properties has become an urgent problem to be solved. Summary of the Invention

[0003] In order to overcome the problems existing in the prior art, the present invention aims to provide a high-strength aluminum-magnesium alloy pre-nickel-plated strip and its production process, which is to form a pre-nickel coating on the aluminum-magnesium alloy surface by nickel plating solution, wherein two kinds of SiO with different particle sizes are added to the nickel plating solution so that the particles are coupled to form a dense single-layer nano-coating, and the SiO with 5-10nm is modified by sodium lauryl sulfate solution while the SiO with 100-200nm is modified by KH550, so that the SiO with two different particle sizes is fully dispersed and uniform, and the particles are coupled to form a more dense nano-coating, and the micro-nano particles are brought into play to enhance the synergistic effect, so that the corrosion resistance, hardness, tensile strength, yield strength and elongation of the nano-nickel coating are significantly improved. In addition, three stress regulators, polylactic acid, sodium o-benzoylsulfonyl imide and saccharin, are added simultaneously, and the internal stress of the nickel coating is eliminated by synergy, the bonding strength between the nickel coating and the substrate is improved, and the nickel coating is made more delicate and uniform, thereby showing better corrosion resistance, tensile strength, yield strength and elongation.

[0004] The object of the present invention is achieved through the following technical solutions:

[0005] A high-strength aluminum-magnesium alloy pre-nickel-plated strip is provided, wherein a nickel layer is pre-plated on the aluminum-magnesium alloy strip, specifically comprising the following steps:

[0006] Step 1: Pretreat the aluminum-magnesium alloy matrix material: dissolve the matrix material with acetone, perform ultrasonic cleaning on the dissolved matrix, wash at room temperature for 5-20 minutes, then use a mixed solution of sodium phosphate and sodium hydroxide to clean dirt and grease on the matrix surface for 5-20 minutes; then pickle with dilute hydrochloric acid for 1-2 minutes.

[0007] Step 2: Prepare a nickel electroplating solution: add 200-500 parts of nickel sulfamate, 100-250 parts of nickel sulfate, 10-20 parts of conductive salt nickel chloride, 12-28 parts of a stress reliever, 1-5 parts of a complexing agent citric acid, 30-50 parts of a buffer, and 20-50 parts of a wetting agent to solvent water, stir and mix thoroughly to obtain 1 L of electroplating solution, then add 15-25 parts of inert nanoparticles and mix evenly, and adjust the pH of the nickel electroplating solution to 3.5 to 4.5.

[0008] Step 3: Place the base material into the pre-nickel plating solution for electroplating to obtain an aluminum-magnesium alloy pre-nickel plating strip having a pre-nickel plating layer.

[0009] Preferably, the inert nanoparticles are surface-modified 5-10 nm SiO2 particles and 100-200 nm SiO2 particles, wherein the mass ratio of the 5-10 nm SiO2 to the 100-200 nm SiO2 is 2-5:1. The surface modification is performed by dispersing the 5-10 nm SiO2 particles in a sodium dodecyl sulfate solution and performing surface chemical modification using ultrasonic dispersion, and dispersing the 100-200 nm SiO2 particles in a KH550 solution and performing surface chemical modification using ultrasonic dispersion, and then mixing and ultrasonically dispersing them. The concentration of the sodium dodecyl sulfate solution is 0.5-1.3 g / L, and the amount of the 5-10 nm SiO2 particles added to the sodium dodecyl sulfate solution is 2-6 g / L; the concentration of the KH550 solution is 0.7-1.8 g / L, and the amount of the 100-200 nm SiO2 particles added to the KH550 solution is 2-5 g / L.

[0010] Preferably, the stress regulator is a mixture of polylactic acid, sodium o-benzoylsulfonimide and saccharin in a mass ratio of (0.5-2): (0.5-1): (0.5-1.5).

[0011] Preferably, the mixture of polylactic acid, sodium o-benzoylsulfonimide and saccharin is composed of a mass ratio of 0.5:0.5:1.

[0012] Preferably, the wetting agent is at least one of cetyltrimethylammonium bromide, sodium lauryl sulfate, sodium dodecylbenzenesulfonate and polyethylene glycol octylphenyl ether.

[0013] Preferably, the buffer comprises at least one of boric acid, sodium tetraborate, sodium oxalate and sodium citrate.

[0014] Preferably, the nickel electroplating solution includes 200-300 parts of nickel sulfamate, 100-150 parts of nickel sulfate, 10-15 parts of conductive salt nickel chloride, 12-20 parts of stress reliever, 1-3.5 parts of complexing agent citric acid, 30-40 parts of buffer, and 20-35 parts of wetting agent. The solution is added to solvent water and stirred thoroughly to obtain 1L of electroplating solution. 15-20 parts of inert nanoparticles are then added and mixed evenly, and the pH of the nickel electroplating solution is adjusted to 3.5 to 4.5.

[0015] Beneficial effects of the present invention:

[0016] 1. Adding chemically modified inert nanoparticles to the nickel plating solution can form a nano-nickel-based composite coating, improving the porosity, corrosion resistance, and mechanical properties of the nickel plating layer. The coupling of two SiO2 particles of different particle sizes forms a dense nano-plating layer, while the synergistic reinforcement effect of micro-nanoparticles is exerted, significantly improving the corrosion resistance, hardness, tensile strength, yield strength, and elongation of the nano-nickel plating layer.

[0017] 2. Furthermore, sodium dodecyl sulfate solution is used to modify 5-10nm SiO2 particles, while KH550 is used to modify 100-200nm SiO2 particles, so that the two SiO2 particles of different particle sizes are fully dispersed and evenly coupled with each other to form a denser nano-plating layer, exerting the synergistic enhancement effect of micro-nanoparticles, and significantly improving the porosity, corrosion resistance, hardness, tensile strength, yield strength and elongation of the nano-nickel plating layer.

[0018] 3. The three stress regulators, polylactic acid, sodium o-benzoylsulfonimide and saccharin, work synergistically to eliminate the internal stress of the nickel plating layer, improve the bonding strength between the nickel plating layer and the substrate, make the nickel plating layer more delicate and uniform, and thus show better tensile strength, yield strength and elongation. DETAILED DESCRIPTION

[0019] The following will clearly and completely describe the technical solutions of the present invention in conjunction with the embodiments. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0020] The present invention will be further explained below with reference to specific embodiments.

[0021] Example 1

[0022] A high-strength aluminum-magnesium alloy pre-nickel-plated strip is provided, wherein a nickel layer is pre-plated on the aluminum-magnesium alloy strip, specifically comprising the following steps:

[0023] Step 1: Pretreat the UM59 aluminum-magnesium alloy strip with a size of 150 mm × 20 mm × 0.17 mm: use acetone to dissolve the base material, perform ultrasonic cleaning on the dissolved material, wash at room temperature for 10 minutes, then use a mixed solution of sodium phosphate and sodium hydroxide to clean the dirt and grease on the surface of the base material for 10 minutes; then pickle with dilute hydrochloric acid for 2 minutes.

[0024] Step 2: Prepare nickel electroplating solution: add 200g of nickel sulfamate, 100g of nickel sulfate, 10g of conductive salt nickel chloride, 12g of stress reliever, 1g of citric acid, 30g of boric acid, and 20g of wetting agent to solvent water, stir and mix thoroughly to obtain 1L of electroplating solution, then add 15g of inert nanoparticles and mix evenly, and adjust the pH of the nickel electroplating solution to 4 with a pH adjuster.

[0025] Step 3: Place the substrate material in the pre-nickel plating solution for electroplating. The nickel plating time is 1 hour and the current density is 1.5A / dm 2 ; A high-strength aluminum-magnesium alloy pre-nickel-plated strip with a nickel layer thickness of 11 μm was obtained.

[0026] The inert nanoparticles are 5 nm SiO2 particles and 100 nm SiO2 particles that have been surface-modified, wherein the mass ratio of 5 nm SiO2 to 100 nm SiO2 is 2:1. The surface modification treatment operation is as follows: 5 nm SiO2 particles are dispersed in a sodium dodecyl sulfate solution to obtain a 3 g / L wet solution, and then ultrasonic dispersion is used to perform surface chemical modification to obtain a modified solution 1; 100 nm SiO2 particles are dispersed in a KH550 solution to obtain a 3 g / L wet solution, and then ultrasonic dispersion is used to perform surface chemical modification to obtain a modified solution 2; and then the modified solution 1 and the modified solution 2 are mixed and ultrasonically dispersed to obtain the obtained solution.

[0027] The stress regulator is a mixture of polylactic acid, sodium o-benzoylsulfonimide and saccharin in a mass ratio of 0.5:0.5:1. The wetting agent is hexadecyltrimethylammonium bromide and polyethylene glycol octylphenyl ether in a mass ratio of 1:1.

[0028] Example 2 KH550 modified to sodium lauryl sulfate solution

[0029] A high-strength aluminum-magnesium alloy pre-nickel-plated strip is provided, wherein a nickel layer is pre-plated on the aluminum-magnesium alloy strip, specifically comprising the following steps:

[0030] Step 1: Pretreat the UM59 aluminum-magnesium alloy strip with a size of 150 mm × 20 mm × 0.17 mm: use acetone to dissolve the base material, perform ultrasonic cleaning on the dissolved material, wash at room temperature for 10 minutes, then use a mixed solution of sodium phosphate and sodium hydroxide to clean the dirt and grease on the surface of the base material for 10 minutes; then pickle with dilute hydrochloric acid for 2 minutes.

[0031] Step 2: Prepare nickel electroplating solution: add 200g of nickel sulfamate, 100g of nickel sulfate, 10g of conductive salt nickel chloride, 12g of stress reliever, 1g of citric acid, 30g of boric acid, and 20g of wetting agent to solvent water, stir and mix thoroughly to obtain 1L of electroplating solution, then add 15g of inert nanoparticles and mix evenly, and adjust the pH of the nickel electroplating solution to 4 with a pH adjuster.

[0032] Step 3: Place the substrate material in the pre-nickel plating solution for electroplating. The nickel plating time is 1 hour and the current density is 1.5A / dm 2 ; A high-strength aluminum-magnesium alloy pre-nickel-plated strip with a nickel layer thickness of 11 μm was obtained.

[0033] The inert nanoparticles are 5nm SiO2 particles and 100nm SiO2 particles that have been surface-modified, wherein the mass ratio of 5nm SiO2 to 100nm SiO2 is 2:1. The surface modification treatment operation is as follows: 5nm SiO2 particles are dispersed in sodium dodecyl sulfate solution to obtain a 3g / L wet solution, and then ultrasonic dispersion is used to perform surface chemical modification to obtain modified solution 1; 100nm SiO2 particles are dispersed in sodium dodecyl sulfate solution to obtain a 3g / L wet solution, and then ultrasonic dispersion is used to perform surface chemical modification to obtain modified solution 2; and then modified solution 1 and modified solution 2 are mixed and ultrasonically dispersed to obtain the obtained solution.

[0034] The stress regulator is a mixture of polylactic acid, sodium o-benzoylsulfonimide and saccharin in a mass ratio of 0.5:0.5:1. The wetting agent is hexadecyltrimethylammonium bromide and polyethylene glycol octylphenyl ether in a mass ratio of 1:1.

[0035] Example 3 Sodium lauryl sulfate solution modified to KH550

[0036] A high-strength aluminum-magnesium alloy pre-nickel-plated strip is provided, wherein a nickel layer is pre-plated on the aluminum-magnesium alloy strip, specifically comprising the following steps:

[0037] Step 1: Pretreat the UM59 aluminum-magnesium alloy strip with a size of 150 mm × 20 mm × 0.17 mm: use acetone to dissolve the base material, perform ultrasonic cleaning on the dissolved material, wash at room temperature for 10 minutes, then use a mixed solution of sodium phosphate and sodium hydroxide to clean the dirt and grease on the surface of the base material for 10 minutes; then pickle with dilute hydrochloric acid for 2 minutes.

[0038] Step 2: Prepare nickel electroplating solution: add 200g of nickel sulfamate, 100g of nickel sulfate, 10g of conductive salt nickel chloride, 12g of stress reliever, 1g of citric acid, 30g of boric acid, and 20g of wetting agent to solvent water, stir and mix thoroughly to obtain 1L of electroplating solution, then add 15g of inert nanoparticles and mix evenly, and adjust the pH of the nickel electroplating solution to 4 with a pH adjuster.

[0039] Step 3: Place the substrate material in the pre-nickel plating solution for electroplating. The nickel plating time is 1 hour and the current density is 1.5A / dm 2 ; A high-strength aluminum-magnesium alloy pre-nickel-plated strip with a nickel layer thickness of 11 μm was obtained.

[0040] The inert nanoparticles are 5 nm SiO2 particles and 100 nm SiO2 particles that have been surface-modified, wherein the mass ratio of 5 nm SiO2 to 100 nm SiO2 is 2:1. The surface modification treatment operation is as follows: 5 nm SiO2 particles are dispersed in KH550 solution to obtain a 3 g / L wet solution, and then ultrasonic dispersion is used to perform surface chemical modification to obtain modified solution 1; 100 nm SiO2 particles are dispersed in KH550 solution to obtain a 3 g / L wet solution, and then ultrasonic dispersion is used to perform surface chemical modification to obtain modified solution 2; and then modified solution 1 and modified solution 2 are mixed and ultrasonically dispersed to obtain the obtained solution.

[0041] The stress regulator is a mixture of polylactic acid, sodium o-benzoylsulfonimide and saccharin in a mass ratio of 0.5:0.5:1. The wetting agent is hexadecyltrimethylammonium bromide and polyethylene glycol octylphenyl ether in a mass ratio of 1:1.

[0042] Comparative Example 1: Only 5 nm SiO2 particles with surface modification were used.

[0043] A pre-nickel-plated aluminum-magnesium alloy strip is provided, wherein a nickel layer is pre-plated on the aluminum-magnesium alloy strip, specifically comprising the following steps:

[0044] Step 1: Pretreat the UM59 aluminum-magnesium alloy strip with a size of 150 mm × 20 mm × 0.17 mm: use acetone to dissolve the base material, perform ultrasonic cleaning on the dissolved material, wash at room temperature for 10 minutes, then use a mixed solution of sodium phosphate and sodium hydroxide to clean the dirt and grease on the surface of the base material for 10 minutes; then pickle with dilute hydrochloric acid for 2 minutes.

[0045] Step 2: Prepare nickel electroplating solution: add 200g of nickel sulfamate, 100g of nickel sulfate, 10g of conductive salt nickel chloride, 12g of stress reliever, 1g of citric acid, 30g of boric acid, and 20g of wetting agent to solvent water, stir and mix thoroughly to obtain 1L of electroplating solution, then add 15g of inert nanoparticles and mix evenly, and adjust the pH of the nickel electroplating solution to 4 with a pH adjuster.

[0046] Step 3: Place the substrate material in the pre-nickel plating solution for electroplating. The nickel plating time is 1 hour and the current density is 1.5A / dm 2 ; Obtain an aluminum-magnesium alloy pre-nickel-plated strip with a nickel layer thickness of 11 μm.

[0047] The inert nanoparticles are 5 nm SiO2 particles that have been surface modified. The surface modification operation is to disperse the 5 nm SiO2 particles in a sodium dodecyl sulfate solution to obtain a 3 g / L wet solution, and then use ultrasonic dispersion to perform surface chemical modification.

[0048] The stress regulator is a mixture of polylactic acid, sodium o-benzoylsulfonimide and saccharin in a mass ratio of 0.5:0.5:1. The wetting agent is hexadecyltrimethylammonium bromide and polyethylene glycol octylphenyl ether in a mass ratio of 1:1.

[0049] The buffer is boric acid. The aluminum-magnesium alloy matrix material is aluminum-magnesium alloy.

[0050] Comparative Example 2: Only 100 nm surface-modified SiO2 particles were used.

[0051] A pre-nickel-plated aluminum-magnesium alloy strip is provided, wherein a nickel layer is pre-plated on the aluminum-magnesium alloy strip, specifically comprising the following steps:

[0052] Step 1: Pretreat the UM59 aluminum-magnesium alloy strip with a size of 150 mm × 20 mm × 0.17 mm: use acetone to dissolve the base material, perform ultrasonic cleaning on the dissolved material, wash at room temperature for 10 minutes, then use a mixed solution of sodium phosphate and sodium hydroxide to clean the dirt and grease on the surface of the base material for 10 minutes; then pickle with dilute hydrochloric acid for 2 minutes.

[0053] Step 2: Prepare nickel electroplating solution: add 200g of nickel sulfamate, 100g of nickel sulfate, 10g of conductive salt nickel chloride, 12g of stress reliever, 1g of citric acid, 30g of boric acid, and 20g of wetting agent to solvent water, stir and mix thoroughly to obtain 1L of electroplating solution, then add 15g of inert nanoparticles and mix evenly, and adjust the pH of the nickel electroplating solution to 4 with a pH adjuster.

[0054] Step 3: Place the substrate material in the pre-nickel plating solution for electroplating. The nickel plating time is 1 hour and the current density is 1.5A / dm 2; Obtain an aluminum-magnesium alloy pre-nickel-plated strip with a nickel layer thickness of 11 μm.

[0055] The inert nanoparticles are 100 nm SiO2 particles that have been surface modified. The surface modification operation is to disperse the 100 nm SiO2 particles in a KH550 solution to obtain a 3 g / L wet solution, and then use ultrasonic dispersion to perform surface chemical modification.

[0056] The stress regulator is a mixture of polylactic acid, sodium o-benzoylsulfonimide and saccharin in a mass ratio of 0.5:0.5:1. The wetting agent is hexadecyltrimethylammonium bromide and polyethylene glycol octylphenyl ether in a mass ratio of 1:1.

[0057] The stress regulator in Comparative Example 3 is a mixture of sodium o-benzoylsulfonimide and saccharin in a mass ratio of 0.5:1.

[0058] A pre-nickel-plated aluminum-magnesium alloy strip is provided, wherein a nickel layer is pre-plated on the aluminum-magnesium alloy strip, specifically comprising the following steps:

[0059] Step 1: Pretreat the UM59 aluminum-magnesium alloy strip with a size of 150 mm × 20 mm × 0.17 mm: use acetone to dissolve the base material, perform ultrasonic cleaning on the dissolved material, wash at room temperature for 10 minutes, then use a mixed solution of sodium phosphate and sodium hydroxide to clean the dirt and grease on the surface of the base material for 10 minutes; then pickle with dilute hydrochloric acid for 2 minutes.

[0060] Step 2: Prepare nickel electroplating solution: add 200g of nickel sulfamate, 100g of nickel sulfate, 10g of conductive salt nickel chloride, 12g of stress reliever, 1g of citric acid, 30g of boric acid, and 20g of wetting agent to solvent water, stir and mix thoroughly to obtain 1L of electroplating solution, then add 15g of inert nanoparticles and mix evenly, and adjust the pH of the nickel electroplating solution to 4 with a pH adjuster.

[0061] Step 3: Place the substrate material in the pre-nickel plating solution for electroplating. The nickel plating time is 1 hour and the current density is 1.5A / dm 2 ; Obtain an aluminum-magnesium alloy pre-nickel-plated strip with a nickel layer thickness of 11 μm.

[0062] The inert nanoparticles are 5 nm SiO2 particles and 100 nm SiO2 particles that have been surface-modified, wherein the mass ratio of 5 nm SiO2 to 100 nm SiO2 is 2:1. The surface modification treatment operation is as follows: 5 nm SiO2 particles are dispersed in a sodium dodecyl sulfate solution to obtain a 3 g / L wet solution, and then ultrasonic dispersion is used to perform surface chemical modification to obtain a modified solution 1; 100 nm SiO2 particles are dispersed in a KH550 solution to obtain a 3 g / L wet solution, and then ultrasonic dispersion is used to perform surface chemical modification to obtain a modified solution 2; and then the modified solution 1 and the modified solution 2 are mixed and ultrasonically dispersed to obtain the obtained solution.

[0063] The stress regulator is a mixture of sodium o-benzoylsulfonimide and saccharin in a mass ratio of 0.5:1. The wetting agent is hexadecyltrimethylammonium bromide and polyethylene glycol octylphenyl ether in a mass ratio of 1:1.

[0064] The stress regulator in Comparative Example 4 is a mixture of polylactic acid and sodium o-benzoylsulfonimide in a mass ratio of 0.5:0.5.

[0065] A pre-nickel-plated aluminum-magnesium alloy strip is provided, wherein a nickel layer is pre-plated on the aluminum-magnesium alloy strip, specifically comprising the following steps:

[0066] Step 1: Pretreat the UM59 aluminum-magnesium alloy strip with a size of 150 mm × 20 mm × 0.17 mm: use acetone to dissolve the base material, perform ultrasonic cleaning on the dissolved material, wash at room temperature for 10 minutes, then use a mixed solution of sodium phosphate and sodium hydroxide to clean the dirt and grease on the surface of the base material for 10 minutes; then pickle with dilute hydrochloric acid for 2 minutes.

[0067] Step 2: Prepare nickel electroplating solution: add 200g of nickel sulfamate, 100g of nickel sulfate, 10g of conductive salt nickel chloride, 12g of stress reliever, 1g of citric acid, 30g of boric acid, and 20g of wetting agent to solvent water, stir and mix thoroughly to obtain 1L of electroplating solution, then add 15g of inert nanoparticles and mix evenly, and adjust the pH of the nickel electroplating solution to 4 with a pH adjuster.

[0068] Step 3: Place the substrate material in the pre-nickel plating solution for electroplating. The nickel plating time is 1 hour and the current density is 1.5A / dm 2 ; Obtain an aluminum-magnesium alloy pre-nickel-plated strip with a nickel layer thickness of 11 μm.

[0069] The inert nanoparticles are 5 nm SiO2 particles and 100 nm SiO2 particles that have been surface-modified, wherein the mass ratio of 5 nm SiO2 to 100 nm SiO2 is 2:1. The surface modification treatment operation is as follows: 5 nm SiO2 particles are dispersed in a sodium dodecyl sulfate solution to obtain a 3 g / L wet solution, and then ultrasonic dispersion is used to perform surface chemical modification to obtain a modified solution 1; 100 nm SiO2 particles are dispersed in a KH550 solution to obtain a 3 g / L wet solution, and then ultrasonic dispersion is used to perform surface chemical modification to obtain a modified solution 2; and then the modified solution 1 and the modified solution 2 are mixed and ultrasonically dispersed to obtain the obtained solution.

[0070] The stress regulator is a mixture of polylactic acid and sodium o-benzoylsulfonimide in a mass ratio of 0.5:0.5. The wetting agent is hexadecyltrimethylammonium bromide and polyethylene glycol octylphenyl ether in a mass ratio of 1:1.

[0071] The performance tests were performed on the aluminum-magnesium alloy pre-nickel-plated strips obtained in Examples 1-3 and Comparative Examples 1-4:

[0072] Composite coating adhesion test: Conduct a 180° bending test in accordance with the national standard GB 232-2010, repeatedly bending 180° until the specimen breaks. If no cracks are found on the coating on the surface of the aluminum-magnesium alloy when inspected at four times the magnification, it is considered excellent. If no cracks are found on the coating on the surface of the aluminum-magnesium alloy when inspected with the naked eye, but a small amount of cracks are found on the coating on the surface of the aluminum-magnesium alloy when inspected at four times the magnification, it is considered qualified. If cracks are found on the coating on the surface of the aluminum-magnesium alloy when inspected with the naked eye, it is considered unqualified.

[0073] Neutral salt spray test: The salt spray test is carried out in accordance with GB / T 10125-2021. The product is placed in a salt spray cycle corrosion test chamber. At a temperature of 35±2°C, a salt solution with a concentration of 50±5g / L is sprayed through a spray device and then settled on the surface of the iron sheet. The salt spray deposition rate is 1.5±0.5mL / (80cm 2 ·h), observe the corrosion of the aluminum-magnesium alloy surface coating after 10 h of corrosion, and record the number of corrosion spots on the surface.

[0074] Hardness test: The coating hardness of the product is tested using a HR-150A Rockwell hardness tester.

[0075] Tensile strength, elongation, and yield strength tests: Tested in accordance with the national standard GB / T 5153-2010.

[0076] Table 1 Properties of aluminum-magnesium alloy pre-nickel-plated strip

[0077]

[0078]

[0079] From the comparison between Example 1 and Comparative Example 1 and Comparative Example 2, it can be seen that compared with Comparative Example 1 in which only 5nm surface-modified SiO2 particles are added and Comparative Example 2 in which only 100nm surface-modified SiO2 particles are added, Example 1 uses both 5nm surface-modified SiO2 particles and 100nm surface-modified SiO2 particles, which can form a dense nano-plating layer through the mutual coupling of two SiO2 particles with different particle sizes, and at the same time exert the synergistic enhancement effect of micro-nanoparticles, so that the corrosion resistance, hardness, tensile strength, yield strength and elongation of the nano nickel plating layer are significantly improved.

[0080] From the comparison of Example 1, Example 2 and Example 3, it can be seen that for the surface modification of SiO2 particles, relative to Example 2 in which sodium lauryl sulfate is used and Example 3 in which KH550 is used, the use of sodium lauryl sulfate solution to modify 5 nm SiO2 particles and the use of KH550 to modify 100 nm SiO2 particles can further improve the corrosion resistance, hardness, tensile strength, yield strength and elongation of the nano nickel plating layer. This may be because after different modifiers are used to modify the 5 nm SiO2 particles and the 100 nm SiO2 particles, the two SiO2 particles with different particle sizes can be coupled with each other to form a denser nano-plating layer.

[0081] From the comparison between Example 1 and Comparative Examples 3 and 4, it can be seen that the compounding of the three stress regulators, polylactic acid, sodium o-benzoylsulfonyl imide and saccharin, can produce a synergistic effect, better eliminate internal stress, and thus improve the bonding strength between the nickel plating layer and the substrate, making the nickel plating layer more delicate and uniform, thereby showing better tensile strength, yield strength and elongation.

[0082] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be considered as equivalent replacement methods and are included in the scope of protection of the present invention.

Claims

1. A high-strength aluminum-magnesium alloy pre-nickel-plated strip, which is a pre-nickel layer on an aluminum-magnesium alloy strip, characterized in that: The raw materials of the nickel pre-plating solution include: 200-500 parts of nickel sulfamate, 100-250 parts of nickel sulfate, 10-20 parts of conductive salt nickel chloride, 12-28 parts of stress reliever, 1-5 parts of complexing agent citric acid, 30-50 parts of buffer, 20-50 parts of wetting agent, and 15-25 parts of inert nanoparticles, wherein the inert nanoparticles are surface-modified 5-10nm SiO2 particles and 100-200nm SiO2 particles, wherein the mass ratio of 5-10nm SiO2 to 100-200nm SiO2 is 2-5:1, The surface-modified inert nanoparticles are modified by dispersing 5-10 nm SiO2 particles in a sodium dodecyl sulfate solution, and then using ultrasonic dispersion to perform surface chemical modification, dispersing 100-200 nm SiO2 particles in a KH550 solution, and then using ultrasonic dispersion to perform surface chemical modification, and then mixing and ultrasonic dispersion to obtain. The stress relieving agent is a mixture of polylactic acid, sodium o-benzoylsulfonyl imide and saccharin in a mass ratio of (0.5-2): (0.5-1): (0.5-1.5).

2. The high-strength aluminum-magnesium alloy pre-nickel-plated strip according to claim 1, characterized in that: The inert nanoparticles are surface-modified SiO2 particles of 5-10 nm and SiO2 particles of 100-200 nm, wherein the mass ratio of the SiO2 of 5-10 nm to the SiO2 of 100-200 nm is 2:

1.

3. The high-strength aluminum-magnesium alloy pre-nickel-plated strip according to claim 1, characterized in that: The stress relieving agent is a mixture of polylactic acid, sodium o-benzoylsulfonyl imide and saccharin in a mass ratio of 0.5:0.5:

1.

4. The high-strength aluminum-magnesium alloy pre-nickel-plated strip according to claim 1, characterized in that: The wetting agent is at least one of cetyltrimethylammonium bromide, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate and polyethylene glycol octylphenyl ether.

5. The high-strength aluminum-magnesium alloy pre-nickel-plated strip according to claim 1, characterized in that: The nickel pre-plating solution comprises 200-300 parts of nickel sulfamate, 100-150 parts of nickel sulfate, 10-15 parts of conductive salt nickel chloride, 12-20 parts of stress reliever, 1-3.5 parts of complexing agent citric acid, 30-40 parts of buffer, 20-35 parts of wetting agent and 15-20 parts of inert nanoparticles.

6. The method for preparing the high-strength aluminum-magnesium alloy pre-nickel-plated strip according to any one of claims 1 to 5, characterized in that: The specific steps include: Step 1: Pre-treat the aluminum-magnesium alloy matrix material: dissolve the matrix material with acetone, perform ultrasonic cleaning on the dissolved matrix material, wash at room temperature for 5-20 minutes, then use a mixed solution of sodium phosphate and sodium hydroxide to clean dirt and grease on the surface of the matrix for 5-20 minutes; then use dilute hydrochloric acid to pickle for 1-2 minutes; Step 2, preparing a nickel electroplating solution: adding nickel sulfamate, nickel sulfate, conductive salt nickel chloride, stress reliever, complexing agent citric acid, buffer, and wetting agent to solvent water, stirring and mixing to obtain 1L of electroplating solution, adding inert nanoparticles and mixing evenly, and adjusting the pH of the nickel electroplating solution to 3.5 to 4.5; Step 3: placing the base material into the pre-nickel plating solution for electroplating to obtain an aluminum-magnesium alloy pre-nickel plating strip having a pre-nickel plating layer.

7. The method for preparing the high-strength aluminum-magnesium alloy pre-nickel-plated strip according to claim 6, characterized in that: The aluminum-magnesium alloy matrix material is UM59.

8. The method for preparing the high-strength aluminum-magnesium alloy pre-nickel-plated strip according to claim 6, characterized in that: The nickel plating layer has a thickness of 10-15 μm.

Citation Information

Patent Citations

  • Method for obtaining micro-nano SiO2 particle containing coating on surface of aluminium and aluminium alloy

    CN102899644A

  • Preparation method of silica particle reinforced nickel-base composite coating for conducting rolls

    CN103031585A

  • Preparation method of composite electronickelling liquid

    CN115161723A

  • Preparation method of nickel aminosulfonate electroplating solution

    CN115161724A

  • Nickel electroplating solution, and preparation method and application of nickel electroplating solution

    CN116926632A