Low-temperature pressureless sintering elargol
By employing a low-temperature, pressureless sintering technology using a multi-solvent compound and sintering aid, combined with nano-silver powder and micron-silver powder, the problem of insufficient adhesion strength of low-temperature, pressureless sintered silver paste on copper substrates has been solved, achieving high electrical and thermal conductivity, making it suitable for packaging high-power electronic devices.
Patent Information
- Application Number
- CN202411278627.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-15
AI Technical Summary
Existing low-temperature pressureless sintering silver paste cannot achieve high-strength sintering on copper substrates, resulting in insufficient bonding strength after sintering. Furthermore, traditional conductive adhesives have low thermal conductivity, which cannot meet the high reliability requirements of high-power electronic devices.
By employing a multi-component solvent compound system and sintering aid, combining nano-silver powder and micron-silver powder, the silver powder particles are fully diffused and fused in a nitrogen atmosphere at 200℃ without pressure or oxygen through low-temperature pressureless sintering technology, forming a high-density interconnected structure. Elemental silver is released at low temperature using a silver precursor to promote sintering.
It achieves high electrical and thermal conductivity on copper substrates, while improving bonding strength and reducing the pressure requirements of the sintering process, making it suitable for packaging high-power electronic devices and solving the problem of potential joint remelting in traditional silver paste at high temperatures.
Smart Images

Figure CN118956290A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic device packaging, and in particular relates to a low-temperature pressureless sintering silver paste. Background Art
[0002] As electronic devices develop towards miniaturization, multifunctionality and high reliability, the requirements for electronic packaging materials are increasing. For example, these materials must be able to operate under high temperature (over 200°C) and high current density conditions. However, traditional tin-lead solder and lead-free solder can no longer meet such usage conditions because their thermal conductivity is usually lower than 60W / m·K, and they are prone to forming holes and poor bonding performance during high and low temperature cycles. Traditional conductive adhesives are mainly composed of organic resins as the bonding phase, which will result in higher organic residues, hindering the movement of electrons between conductive particles, resulting in the thermal conductivity of conductive adhesives being usually lower than 30W / m·K.
[0003] Low-temperature pressureless sintering silver paste containing nanosilver has excellent electrical and thermal conductivity, low organic residue, and can withstand an operating temperature of more than 500°C after sintering. It can effectively avoid the problem of joint remelting during subsequent processing and use of electronic devices. Therefore, low-temperature pressureless sintering silver paste is particularly suitable for the packaging of high-power electronic devices. However, there are still some problems with low-temperature pressureless sintering silver paste. For example, high-power devices usually use gold as the substrate for chip bonding, but the cost of gold is relatively high. In view of the price advantage of copper and its ability to meet the electronic properties required by high-power devices, it has become a trend to replace gold with copper. However, high-strength sintering between copper substrate and silver paste usually requires pressure sintering technology, which not only requires expensive professional equipment, but also may cause damage to the chip, thereby limiting its scope of application. In addition, most of the current low-temperature pressureless sintering silver technologies require sintering temperatures generally higher than 220°C, and many even exceed 250°C. This not only exceeds the temperature resistance limit of many printed circuit boards and other electronic materials, but may also lead to a sharp increase in internal stress due to mismatched thermal expansion coefficients, thereby increasing the risk of failure and seriously affecting the reliability of silver glue sintered joints. The existing low-temperature pressureless sintering silver glue on the market cannot achieve high-strength sintering on metal copper substrates, resulting in insufficient bonding strength after sintering, which also limits its application range. For this reason, a low-temperature pressureless sintering silver glue is proposed. Summary of the invention
[0004] The purpose of the present invention is to provide a low-temperature pressureless sintering silver paste, aiming to solve the problems raised in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A low-temperature pressureless sintering silver paste comprises the following raw materials in parts by weight: 50-95 parts of conductive filler, 1-30 parts of organic carrier, 0.1-10 parts of sintering aid and 0-5 parts of rheology modifier.
[0007] Furthermore, the conductive filler is one or more of micron silver powder, nano silver powder, aluminum powder, nickel powder and silver precursor; the micron silver powder is in the shape of flakes or spheres, with an average particle size of 1-10um; the nano silver powder is in the shape of spheres, with an average particle size of 100-500nm and a specific surface area of 0.5-7m 2 / g; the aluminum powder and the nickel powder are in the shape of one or more of flake, spherical and dendritic, with an average particle size of 1-5um; the silver precursor is a silver compound that decomposes at a temperature below 200°C and releases elemental silver, and is one or more of silver carbonate, silver lactate, silver formate, silver citrate and silver oxide (such as AgO or Ag2O).
[0008] Further, the organic carrier is a mixture of acrylate, cellulose and phenoxy resin dissolved in an organic solvent, the acrylate is one or more of diethylene glycol diacrylate, dipentaerythritol hexaacrylate, isobornyl acrylate, acryloyl morpholine and tetrahydrofuran acrylate; the cellulose is one or more of trade names such as HHBER250, HBR250, MBR250, HE10K, EASTMAN CAB 381-0.5 and CA-398-3; the phenoxy resin is one or more of trade names such as Araldite488E-32, Araldite 488N-40, DER 686MK40, PKHS-30PMA, PKHB Pellets, PKHHPellets, Epokote-1256, Epokote-4257, YP-50, YP-50S and YP-70; the organic solvent is one or more of pineol, methanol, ethylene glycol, n-hexanol, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, polyhydroxystearin, diethylene glycol butyl ether, diglycidyl hexahydrophthalate, diethylene glycol butyl ether acetate, tripropylene glycol monomethyl ether, tripropylene glycol butyl ether, ethyl 2-isobutoxybenzoate, 2-ethyl-1,3-hexanediol, dipropylene glycol methyl ether acetate, diethyl adipate, dibasic ester, ethyl benzoate, butyl carbitol acetate, propylene glycol methyl ether acetate, ethylene glycol carbonate and diethylhexyl maleate.
[0009] Further, the sintering aid is one or more of aluminum triformate, ferrous phosphate, di(1,1-dimethylpropyl)peroxide, di-tert-butyl peroxide, benzoyl peroxide, diisobutyryl peroxide, isopropyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, di-n-propyl peroxydicarbonate, tert-amyl peroxyneodecanoate, di-(3,5,5-trimethylhexanoyl)-peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, 1,1-di-(tert-butylperoxy)-3,3,5-trimethylcyclohexane and 1,1-di-(tert-butylperoxy)-cyclohexane.
[0010] Further, the rheology modifier is one or more of trade names such as BYK111, BYK110, BYK310, BYK106, BYK-7410ET, fumed silica and carbon nanotubes; the fumed silica is one or more of AEROSIL R202, AEROSIL R974, AEROSIL 200, AEROSIL 380, Cabot TS610, Cabot TS720, Cabot LM-150, Wacker H15, Wacker H18, Wacker N20, Wacker V15, Wacker H20 and Wacker H30.
[0011] A method for preparing the low-temperature pressureless sintering silver paste according to the above-mentioned method is characterized by comprising the following steps:
[0012] First, the organic carrier components are weighed by weight percentage and mixed evenly; then the rheology modifier and the conductive filler are weighed by weight percentage and added to the organic carrier, stirred with a homogenizer, and then ground with a three-roll grinder to achieve a fineness of 2.3-8um, and filtered through a filter; the ground and filtered silver paste is placed at room temperature and vacuum degassed for 15 minutes to obtain low-temperature pressureless sintered silver paste.
[0013] Furthermore, the speed of the homogenizer is controlled at 1000-2000 rpm, the stirring time is 1-5 minutes, and the stirring temperature is maintained below 40°C.
[0014] Furthermore, the mesh size of the filter is 300-600 meshes.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] 1. The low-temperature pressureless sintering silver paste of the present invention can be sintered at 200°C in a pressureless, oxygen-free nitrogen atmosphere. After sintering, the bonding strength to the metal silver and metal copper substrates is greater than 25MPa. At the same time, it has high electrical conductivity (volume resistivity <10μΩ·cm) and high thermal conductivity (thermal conductivity >100W / m·K). In addition, the silver paste is halogen-free and environmentally friendly, and the porosity of the product after sintering is low, which further improves the overall performance and reliability of the product and is suitable for solving the heat dissipation problem of high-power electronic device packaging.
[0017] 2. The low-temperature pressureless sintering silver paste of the present invention realizes the step-by-step control of solvent volatilization through an innovative multi-solvent compounding system, promotes the full diffusion and fusion of silver powder particles during the sintering process, builds a more compact interconnected structure, and significantly enhances the reliability of sintered silver during use. At the same time, the low-temperature pressureless sintering silver paste is composed of a compound of nano silver powder and micron silver powder. Its sintering process uses nano silver powder with high surface energy as the main driving force, combined with the synergistic effect of sintering aids and silver precursors, and successfully achieves low-temperature sintering in a pressureless, oxygen-free nitrogen environment at 200°C, reducing the requirements for sintering auxiliary pressure during the sintering process, and achieving the effect of low-temperature pressureless sintering. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the SEM image of the silver carbonate added in Example 1.
[0019] Figure 2 The SEM images of silver oxide added in Examples 2-4 and Comparative Example 2 are shown.
[0020] Figure 3 This is the SEM image of the nano-spherical silver powder with a size of 150 nm added in Example 2.
[0021] Figure 4 This is an X-ray image of the sintered body of Example 4.
[0022] Figure 5 This is a SEM image of the microstructure of the cross section of the sintered body of Example 4.
[0023] Figure 6 This is a SEM image of the microstructure of the cross section of the sintered body of Comparative Example 2. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0025] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.
[0026] Embodiment 1: A low-temperature pressureless sintering silver paste, the preparation method of which comprises the following steps:
[0027] (1) Weighing 0.3 g of terpineol, 0.1 g of diethylene glycol butyl ether acetate, 0.2 g of 2-ethyl-1,3-hexanediol and 0.4 g of diethylhexyl maleate to prepare an organic carrier mixture, and stirring the mixture at a speed of 1200 rpm for 2 minutes using a homogenizer, and controlling the temperature to be below 40° C. during the stirring process;
[0028] (2) Add 0.05 g of rheology modifier BYK111 to step (1), and stir at 1200 rpm for 2 minutes using a homogenizer. During the stirring process, the temperature is controlled below 40° C.
[0029] (3) adding 8.2 g of nano-spherical silver powder (prepared in-house) with a size of 300 nm and 0.65 g of silver carbonate (prepared in-house) with a size of 400 nm to the mixture in step (2), and stirring the mixture at a speed of 1500 rpm for 3 minutes using a homogenizer, with the temperature being controlled below 40° C. during the stirring process;
[0030] (4) dispersing the slurry obtained in step (3) seven times using a three-roll mill, and controlling the temperature below 40° C. during the dispersing process;
[0031] (5) The slurry dispersed in step (4) was filtered twice with a 500-mesh filter, and then placed in a vacuum degassing machine for vacuum degassing at room temperature for 15 minutes to obtain the low-temperature pressureless sintering silver paste.
[0032] Embodiment 2: A low-temperature pressureless sintering silver paste, the preparation method of which comprises the following steps:
[0033] (1) Weighing 0.5 g of terpineol, 0.15 g of diethylene glycol butyl ether acetate and 0.35 g of butyl carbitol acetate to prepare an organic carrier mixture, stirring the mixture at a speed of 1200 rpm for 2 minutes using a homogenizer, and controlling the temperature to be below 40° C. during the stirring process;
[0034] (2) adding 0.02 g of rheology modifier Cabot TS720 to step (1), stirring at 1200 rpm for 2 minutes using a homogenizer, and controlling the temperature below 40° C. during the stirring process;
[0035] (3) adding 3.0 g of 2 μm-sized micron-flaky silver powder, 5.1 g of 150 nm-sized nano-spherical silver powder (self-made) and 0.6 g of silver oxide (self-made) to the mixture in step (2), and stirring the mixture at 1500 rpm for 3 minutes using a homogenizer, with the temperature being controlled below 40° C. during the stirring process;
[0036] (4) dispersing the slurry obtained in step (3) seven times using a three-roll mill, and controlling the temperature below 40° C. during the dispersing process;
[0037] (5) The slurry dispersed in step (4) was filtered twice with a 500-mesh filter, and then placed in a vacuum degassing machine for vacuum degassing at room temperature for 15 minutes to obtain the low-temperature pressureless sintering silver paste.
[0038] Embodiment 3: A low-temperature pressureless sintering silver paste, the preparation method of which comprises the following steps:
[0039] (1) 0.005 g of EASTMAN CAB 381-0.5, 0.295 g of terpineol, 0.15 g of polyhydroxy stearate, 0.3 g of 2-ethyl-1,3-hexanediol and 0.25 g of diethylene glycol butyl ether acetate were weighed to prepare an organic carrier mixture, and the mixture was stirred at a speed of 1200 rpm for 2 minutes using a homogenizer, and the temperature was controlled below 40° C. during the stirring process;
[0040] (2) Add 0.2 g of fumed silica AEROSIL R202 to step (1), and stir the mixture at 1200 rpm for 2 minutes using a homogenizer. During the stirring process, the temperature is controlled below 40° C.
[0041] (3) adding 4.9 g of 2 μm-sized micron-flaky silver powder, 2.1 g of 450 nm-sized nano-spherical silver powder, 0.4 g of silver oxide (homemade) and 0.1 g of aluminum triformate to the mixture in step (2), and stirring the mixture at 1500 rpm for 3 minutes using a homogenizer, with the temperature being controlled below 40° C. during the stirring process;
[0042] (4) dispersing the slurry obtained in step (3) seven times using a three-roll mill, and controlling the temperature below 40° C. during the dispersing process;
[0043] (5) The slurry dispersed in step (4) was filtered twice with a 500-mesh filter, and then placed in a vacuum degassing machine for vacuum degassing at room temperature for 15 minutes to obtain the low-temperature pressureless sintering silver paste.
[0044] Embodiment 4: A low-temperature pressureless sintering silver paste, the preparation method of which comprises the following steps:
[0045] (1) Weighing 0.15 g of diglycidyl hexahydrophthalate, 0.15 g of diethylene glycol butyl ether acetate and 0.7 g of butyl carbitol acetate to prepare an organic carrier mixture, stirring the mixture at a speed of 1200 rpm for 2 minutes using a homogenizer, and controlling the temperature to be below 40° C. during the stirring process;
[0046] (2) adding 0.05 g of rheology modifier BYK-7410ET to step (1), stirring at 1200 rpm for 2 minutes using a homogenizer, and controlling the temperature below 40° C. during the stirring process;
[0047] (3) adding 8.0 g of nano-spherical silver powder with a size of 400 nm, 1.0 g of silver oxide (homemade) and 0.2 g of benzoyl peroxide to the mixture in step (2), and stirring the mixture at a speed of 1500 rpm for 3 minutes using a homogenizer, with the temperature being controlled below 40° C. during the stirring process;
[0048] (4) dispersing the slurry obtained in step (3) seven times using a three-roll mill, and controlling the temperature below 40° C. during the dispersing process;
[0049] (5) The slurry dispersed in step (4) was filtered twice with a 500-mesh filter, and then placed in a vacuum degassing machine for vacuum degassing at room temperature for 15 minutes to obtain the low-temperature pressureless sintering silver paste.
[0050] Comparative Example 1: A low-temperature pressureless sintering silver paste, the preparation method of which comprises the following steps:
[0051] (1) Weighing 0.3 g of terpineol, 0.1 g of diethylene glycol butyl ether acetate, 0.2 g of 2-ethyl-1,3-hexanediol and 0.4 g of diethylhexyl maleate to prepare an organic carrier mixture, and stirring the mixture at a speed of 1200 rpm for 2 minutes using a homogenizer, and controlling the temperature to be below 40° C. during the stirring process;
[0052] (2) Add 0.05 g of rheology modifier BYK111 to step (1), and stir at 1200 rpm for 2 minutes using a homogenizer. During the stirring process, the temperature is controlled below 40° C.
[0053] (3) adding 8.2 g of 300 nm nano-spherical silver powder (homemade) to step (2), stirring the mixture at 1500 rpm for 3 minutes using a homogenizer, and controlling the temperature below 40° C. during the stirring process;
[0054] (4) dispersing the slurry obtained in step (3) seven times using a three-roll mill, and controlling the temperature below 40° C. during the dispersing process;
[0055] (5) The slurry dispersed in step (4) was filtered twice with a 500-mesh filter, and then placed in a vacuum degassing machine for vacuum degassing at room temperature for 15 minutes to obtain the low-temperature pressureless sintering silver paste.
[0056] Comparative Example 2: A low-temperature pressureless sintering silver paste, the preparation method of which comprises the following steps:
[0057] (1) Weighing 0.15 g of diglycidyl hexahydrophthalate, 0.15 g of diethylene glycol butyl ether acetate and 0.7 g of butyl carbitol acetate to prepare an organic carrier mixture, stirring the mixture at a speed of 1200 rpm for 2 minutes using a homogenizer, and controlling the temperature to be below 40° C. during the stirring process;
[0058] (2) adding 0.05 g of rheology modifier BYK-7410ET to step (1), stirring at 1200 rpm for 2 minutes using a homogenizer, and controlling the temperature below 40° C. during the stirring process;
[0059] (3) adding 8.0 g of nano-spherical silver powder with a size of 400 nm and 1.0 g of silver oxide (homemade) to the mixture in step (2), and stirring the mixture at a speed of 1500 rpm for 3 minutes using a homogenizer, with the temperature being controlled below 40° C. during the stirring process;
[0060] (4) dispersing the slurry obtained in step (3) seven times using a three-roll mill, and controlling the temperature below 40° C. during the dispersing process;
[0061] (5) The slurry dispersed in step (4) was filtered twice with a 500-mesh filter, and then placed in a vacuum degassing machine for vacuum degassing at room temperature for 15 minutes to obtain the low-temperature pressureless sintering silver paste.
[0062] like Figure 1 Shown is the SEM image of the silver carbonate added in Example 1.
[0063] like Figure 2 Shown are SEM images of silver oxide added in Examples 2-4 and Comparative Example 2.
[0064] like Figure 3 Shown is a SEM image of nano-spherical silver powder with a size of 150 nm added in Example 2.
[0065] like Figure 4 Shown is an X-ray image of the sintered body of Example 4.
[0066] The performance tests were conducted on the low-temperature pressureless sintering silver pastes prepared in Examples 1-4 and Comparative Examples 1 and 2:
[0067] (1) Volume resistivity: Silver paste is coated on a glass slide into lines with a length of 50 mm, a width of 5 mm, and a thickness of 30 μm. The lines are placed in a nitrogen oven for sintering and curing. After being taken out and cooled to room temperature, the resistance of the lines is measured with a low resistance tester and the volume resistivity is calculated. The sintering and curing process includes: heating from room temperature to 150°C in 20 minutes, keeping the temperature at 150°C for 60 minutes; then heating to 200°C in 15 minutes and keeping the temperature for 90 minutes.
[0068] (2) Adhesion strength: Use a dispensing machine to apply the prepared silver glue on the test substrate, attach the chip, put it in a nitrogen oven for sintering and curing, and then take it out to test the adhesion performance at room temperature and the adhesion performance and thermal conductivity at high temperature (260°C). The test substrate is chip: 2*2mm silver-plated chip; substrate: copper / silver-plated, PPF (Pre-Plating frame Finish) nickel-palladium-gold / nickel-platinum-gold substrate.
[0069] (3) Observation of holes and sintering necks: The solidified chip and substrate are placed under the X-ray equipment for observation. At the same time, they are sliced and their cross sections are observed under a scanning electron microscope (SEM) to further observe the appearance of holes and sintering necks.
[0070] The test results are shown in Table 1.
[0071] Table 1 Test results of low temperature pressureless sintering silver paste prepared in Examples 1-4 and Comparative Examples 1 and 2
[0072]
[0073]
[0074] As shown in Table 1, compared with Example 1, Comparative Example 1 has poor electrical conductivity, thermal conductivity and bonding performance on the test substrate without adding silver carbonate, especially on the copper-plated substrate. This is because the compatibility between silver and copper is poor. When no additional material with bonding effect is added, the conductive silver paste with only silver powder added has insufficient adhesion on the copper substrate; due to the insufficient sintering of silver powder, the gap between silver powder is large, the compactness cannot be guaranteed, the conductive layer formed after sintering has limited adhesion to the substrate, and gaps are easily formed between the conductive layers, affecting the electrical and thermal conductivity. In contrast, Example 1 with the addition of silver carbonate begins to decompose elemental silver when a certain temperature is reached, which promotes the sintering of nano silver powder, improves the compactness of the silver paste and the bonding effect with the substrate.
[0075] Compared with Comparative Example 1, Comparative Example 2 adds silver salt silver oxide, and the electrical conductivity, thermal conductivity and bonding properties on the silver-plated and copper-plated substrates are significantly improved. Figure 5 and Figure 6It can be seen that Example 4, on the basis of adding silver salt silver oxide, further adds a sintering aid benzoyl oxide, which can not only effectively treat the surface of the silver-plated and copper-plated substrates once, but also further promote the reduction of silver oxide during the curing process, generate more elemental silver, and promote the sintering of nano silver powder, thereby improving the density of the silver paste and the bonding effect with the substrate, and then making the silver powder sintered more fully during the curing process, showing better electrical conductivity, thermal conductivity and bonding performance than Comparative Example 2.
[0076] The above are only preferred embodiments of the present invention. It should be pointed out that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention. These should also be regarded as the protection scope of the present invention. These will not affect the effect of the implementation of the present invention and the practicality of the patent.
Claims
1. A low-temperature pressureless sintering silver paste, characterized in that: The low-temperature pressureless sintering silver paste comprises the following raw materials in parts by weight: 50-95 parts of conductive filler, 1-30 parts of organic carrier, 0.1-10 parts of sintering aid and 0-5 parts of rheology modifier.
2. The low temperature pressureless sintering silver paste according to claim 1, characterized in that: The conductive filler is one or more of micron silver powder, nano silver powder, aluminum powder, nickel powder and silver precursor; the micron silver powder is in the shape of flakes or spheres, with an average particle size of 1-10um; the nano silver powder is in the shape of spheres, with an average particle size of 100-500nm and a specific surface area of 0.5-7m 2 / g; the shapes of the aluminum powder and the nickel powder are one or more of flake, spherical and dendritic, with an average particle size of 1-5um; the silver precursor is one or more of silver carbonate, silver lactate, silver formate, silver citrate and silver oxide.
3. The low temperature pressureless sintering silver paste according to claim 1, characterized in that: The organic carrier is a mixture of acrylate, cellulose and phenoxy resin dissolved in an organic solvent, wherein the acrylate is one or more of diethylene glycol diacrylate, dipentaerythritol hexaacrylate, isobornyl acrylate, acryloyl morpholine and tetrahydrofuran acrylate; the cellulose is one or more of HHBER250, HBR250, MBR250, HE10K, EASTMAN CAB 381-0.5 and CA-398-3; the phenoxy resin is Araldite 488E-32, Araldite 488N-40, DER 686MK40, PKHS-30PMA, PKHB Pellets, PKHH The organic solvent is one or more of terpineol, methanol, ethylene glycol, n-hexanol, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, polyhydroxystearin, diethylene glycol butyl ether, diglycidyl hexahydrophthalate, diethylene glycol butyl ether acetate, tripropylene glycol monomethyl ether, tripropylene glycol butyl ether, ethyl 2-isobutoxybenzoate, 2-ethyl-1,3-hexanediol, dipropylene glycol methyl ether acetate, diethyl adipate, dibasic ester, ethyl benzoate, butyl carbitol acetate, propylene glycol methyl ether acetate, ethylene glycol carbonate and diethylhexyl maleate.
4. The low temperature pressureless sintering silver paste according to claim 1, characterized in that: The sintering aid is one or more of aluminum triformate, ferrous phosphate, di(1,1-dimethylpropyl)peroxide, di-tert-butyl peroxide, benzoyl peroxide, diisobutyryl peroxide, isopropyl peroxyneodecanoate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, di-n-propyl peroxydicarbonate, tert-amyl peroxyneodecanoate, di-(3,5,5-trimethylhexanoyl)-peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxyisobutyrate, 1,1-di-(tert-butylperoxy)-3,3,5-trimethylcyclohexane and 1,1-di-(tert-butylperoxy)-cyclohexane.
5. The low temperature pressureless sintering silver paste according to claim 1, characterized in that: The rheology modifier is one or more of BYK111, BYK110, BYK310, BYK106, BYK-7410ET, fumed silica and carbon nanotubes; the fumed silica is one or more of AEROSIL R202, AEROSIL R974, AEROSIL 200, AEROSIL 380, Cabot TS610, Cabot TS720, Cabot LM-150, Wacker H15, Wacker H18, Wacker N20, Wacker V15, Wacker H20 and Wacker H30.
6. A method for preparing low-temperature pressureless sintering silver paste according to any one of claims 1 to 5, characterized in that: The following steps are involved: First, the organic carrier components are weighed by weight percentage and mixed evenly; then the rheology modifier and the conductive filler are weighed by weight percentage and added to the organic carrier, stirred with a homogenizer, and then ground with a three-roll grinder to achieve a fineness of 2.3-8um, and filtered through a filter; the ground and filtered silver paste is placed at room temperature and vacuum degassed for 15 minutes to obtain low-temperature pressureless sintered silver paste.
7. The preparation method according to claim 6, characterized in that: The speed of the homogenizer is controlled at 1000-2000 rpm, the stirring time is 1-5 minutes, and the stirring temperature is maintained below 40°C.
8. The preparation method according to claim 6, characterized in that: The mesh number of the filter is 300-600 meshes.
Citation Information
Cited By
Pressureless sintering silver-copper compound adhesive suitable for sintering interconnection of copper-gold-silver heterogeneous interface and preparation method
CN120718566A
A pressureless sintering silver copper compound adhesive suitable for copper-gold-silver heterogeneous interface sintering interconnection and a preparation method thereof
CN120718566B
Nano sintered silver paste and preparation method thereof
CN121662482A
Nanosintered silver paste and preparation method thereof
CN121662482B