Halogen-free flame-retardant polyurethane cable sheath material and preparation method
By using modified boron nitride nanosheets and ferrite powder in polyester TPU cable sheaths, combined with materials such as sodium lignosulfonate-maleic anhydride graft copolymer, to form a highly efficient flame-retardant polymer, the problem is solved The problem of poor flame retardant performance of polyester TPU has been achieved. It has achieved halogen-free, efficient flame retardant and improved mechanical properties, and is suitable for a variety of applications.
Patent Information
- Application Number
- CN202410708731.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-03
AI Technical Summary
The existing polyester TPU cable sheath has poor flame retardant properties. The oxygen index (LOI) without flame retardant treatment is only about 17%, which cannot meet the fire retardant requirements. Moreover, traditional flame retardant methods will release toxic smoke and gases. , there are fire hazards and environmental hazards.
It uses thermoplastic polyurethane elastomer, linear low-density polyethylene and EPDM rubber as the base material, and introduces modified boron nitride nanosheets and ferrite powder, grafted by sodium lignosulfonate-maleic anhydride. Copolymer, dimethylaminoethyl acrylate and propylene phosphate modify boron nitride to form a transition layer and flame retardant polymer, improve flame retardant performance and compatibility, reduce interface defects, and promote the formation of carbon layer to achieve efficient flame retardancy .
It achieves efficient flame retardant properties of halogen-free flame-retardant polyurethane cable sheath materials, reduces the release of toxic smoke, improves mechanical strength and toughness, is suitable for industrial, agricultural and household applications, and reduces fire hazards.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of polymer materials for cables, and in particular to a halogen-free flame-retardant polyurethane cable sheath material and a preparation method thereof. Background Art
[0002] The existing cable sheaths made of polyester TPU have poor flame retardancy as an organic polymer. Therefore, the oxygen index (LOI) of polyester TPU without flame retardant treatment is only about 17%, which is far from the fire retardant requirements required for the use of materials. This poses a great fire hazard in its application sites. The existing method of flame retardant modification of polyester TPU is usually to add non-reactive halogenated compounds as flame retardants to TPU, but after burning, it will release a large amount of smoke and toxic and harmful gases, which will not only suffocate people, but also damage equipment and cause serious harm to the environment and organisms. At the same time, in the actual preparation process, the poor compatibility and weak bonding between substances will also cause the problem of reduced flame retardancy of polyurethane. How to optimize the flame retardant properties of thermoplastic polyurethane elastomer cable outer sheath materials is a problem that the cable manufacturing and processing industry needs to solve. Summary of the invention
[0003] In order to solve the above technical problems, a halogen-free flame retardant polyurethane cable sheath material with excellent flame retardant properties, which meets environmental protection requirements, is strictly halogen-free, and can be widely used is developed. The present application provides a halogen-free flame retardant polyurethane cable sheath material and a preparation method.
[0004] In the first aspect, the present application provides a halogen-free flame-retardant polyurethane cable sheath material, comprising the following raw materials in parts by weight: 80-110 parts of thermoplastic polyurethane elastomer, 25-38 parts of linear low-density polyethylene, 10-15 parts of ethylene propylene rubber, 5-8 parts of compatibilizer, 0.1-1 part of antioxidant, 0.5-1 part of cross-linking agent, and 6-11 parts of filler-type flame retardant; the filler-type flame retardant is modified boron nitride, and the modified boron nitride is prepared by modifying boron nitride nanosheets with sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate.
[0005] By adopting the above technical scheme, the present application uses thermoplastic polyurethane elastomer, linear low-density polyethylene and ethylene propylene diene monomer rubber for compounding, and uses them as the base material of the cable sheath. The thermoplastic polyurethane elastomer has a flexible segment structure, and after adding it, the cable sheath has good ductility, and when subjected to external force, it can well offset the external force internally and digest the stress internally, thereby achieving high resistance of the cable sheath material. Linear low-density polyethylene has a high softening temperature and melting temperature, and can maintain good physical properties in a wide temperature range. At the same time, LLDPE (linear low-density polyethylene) also has excellent environmental stress cracking resistance and impact strength resistance. After adding it, it can also significantly improve the toughness and mechanical strength of the cable sheath. The present application introduces modified boron nitride nanosheets into polyurethane. The modified boron nitride nanosheets are modified by copolymerization of sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate, and a layer of organic polymer is formed on the surface of the boron nitride nanosheets, thereby forming a transition layer between the modified boron nitride nanosheets and the polyurethane matrix material, reducing interface defects, so that the modified boron nitride nanosheets can better play a reinforcing role; on the other hand, the transition layer also improves the compatibility of the modified boron nitride nanosheets in the matrix material. Sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate are cross-linked and polymerized on the surface of boron nitride nanosheets to form a layer of flame retardant polymer to coat the boron nitride nanosheets, thereby further strengthening the flame retardant properties of the filler. The IFR intumescent flame retardant system formed in the flame retardant polymer can promote the formation of a carbon layer when the polyurethane sheath material burns. The physical barrier effect of the boron nitride nanosheets makes the cable sheath material have good anti-dripping performance. At the same time, the boron nitride nanosheets can play a good supporting role as a filler in the polyurethane sheath matrix material, which can inhibit the dripping phenomenon during the combustion process. In addition, the sodium lignin sulfonate connected to the flame retardant polymer as a carbon source of the intumescent flame retardant makes the composite material have a better carbonization effect under high temperature conditions, forming a stable and dense carbon layer structure during the combustion process, while achieving high-efficiency flame retardancy and reducing the release of toxic smoke.
[0006] Furthermore, the compatibilizer is selected from one or more of POE-g-MAH (maleic anhydride grafted octene copolymer), POP-g-MAH (polypropylene terephthalate grafted maleic anhydride), and MAH-g-SBS (maleic anhydride grafted styrene-butadiene-styrene block copolymer).
[0007] The use of the above-mentioned compatibilizer in the technical solution of the present application can improve the bonding between different types of matrix materials and between the matrix material and the filler; in addition, the anhydride groups in the compatibilizer can react with the active groups in the flame-retardant polymer layer on the surface of the modified boron nitride nanosheets to form bonds, forming a transition layer between the modified boron nitride nanosheets and the polyurethane matrix material, reducing interface defects, and further improving the bonding between the matrix material and the filler, so that the modified boron nitride can better play its flame retardant and reinforcing role.
[0008] Furthermore, the antioxidant includes one or more of hindered phenol antioxidants, aromatic amine antioxidants, and phosphite antioxidants.
[0009] Furthermore, the propylene phosphate includes one or more of dimethyl allyl phosphate, methacrylate alkoxy phosphate, and diethyl isopropylene phosphate.
[0010] Propylene phosphate participates in the modification reaction of boron nitride nanosheets, so that the polymer coated with boron nitride nanosheets has a large number of phosphate groups, providing an acid source for the IFR intumescent flame retardant system, and can also participate in the polymerization reaction to further improve the degree of polymerization and cross-linking of the organic polymer coated with the boron nitride nanosheets.
[0011] Furthermore, the preparation method of the modified boron nitride comprises the following steps:
[0012] 1) Mix boron nitride nanosheets, deionized water and glacial acetic acid, disperse by ultrasonication, add Tris alcohol aqueous solution, heat to 50-65°C, stir to react, cool, filter to obtain the residue, wash with water, and dry to obtain an intermediate material;
[0013] 2) Add an organic solvent into a reaction vessel, add benzoyl peroxide, sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate under nitrogen protection, stir and react for 2-3 hours, add the intermediate material prepared in step 1), stir and react for 2-5 hours, filter, wash the filter residue, and dry to obtain modified boron nitride.
[0014] Furthermore, the weight ratio of boron nitride nanosheets, Tris (trishydroxymethylaminomethane), sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate is 10-20:18-32:8-15:12-19:18-32.
[0015] Preferably, the preparation method of the modified boron nitride comprises the following steps:
[0016] 1) Boron nitride nanosheets, deionized water and glacial acetic acid are mixed, ultrasonically dispersed, and a 20 wt% alcohol aqueous solution of Tris is added, wherein the volume ratio of ethanol to water is 1:1; the temperature is raised to 60°C, stirred for reaction for 3 hours, cooled, filtered to obtain the residue, washed with water, and dried at 60°C to obtain an intermediate material;
[0017] 2) Add an organic solvent to a reaction vessel, raise the temperature to 80°C under nitrogen protection, add benzoyl peroxide, stir for 5 minutes, add sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate, stir and react for 3 hours at 80°C, add the intermediate material prepared in step 1), stir and react for 4 hours, filter, wash the filter residue, and dry to obtain modified boron nitride; wherein the organic solvent is xylene, and the weight ratio of the organic solvent to the intermediate material is 6:1; the amount of the initiator benzoyl peroxide is 2% of the total amount of the sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate.
[0018] The weight ratio of boron nitride nanosheets, Tris, sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate is 12:30:9:18:30.
[0019] Furthermore, the preparation method of the sodium lignin sulfonate-maleic anhydride graft copolymer comprises the following steps:
[0020] Sodium lignin sulfonate was dissolved in distilled water, sodium bisulfite and ammonium persulfate were added, and stirred for 5 minutes to prepare a premixed solution; maleic anhydride and 70wt% ammonia water were mixed in equal weight ratios to prepare an ammoniated mixed solution, and the ammoniated mixed solution was added dropwise to the premixed solution, stirred and reacted at 45°C for 1.5 hours, precipitated with hydrochloric acid, filtered, washed and dried at 45°C to prepare a sodium lignin sulfonate-maleic anhydride graft copolymer. The weight ratio of sodium lignin sulfonate, distilled water, sodium bisulfite, ammonium persulfate and maleic anhydride was 1:5:0.25:0.5:1.
[0021] The sodium lignin sulfonate-maleic anhydride graft copolymer added in the present invention works together with other raw materials to significantly improve the thermal stability of the cable sheath material. In addition, the sodium lignin sulfonate in the sodium lignin sulfonate-maleic anhydride graft copolymer serves as a carbon source for the intumescent flame retardant, so that the composite material has a better carbonization effect under high temperature conditions and forms a stable and dense carbon layer structure during the combustion process.
[0022] Furthermore, the raw materials of the halogen-free flame-retardant polyurethane cable sheath material also include 2-5 parts by weight of a synergist, and the synergist is ferrite powder.
[0023] Preferably, the raw materials of the halogen-free flame-retardant polyurethane cable sheath material further include 2.5 parts by weight of a synergist, and the synergist is ferrite powder.
[0024] Specifically, the ferrite powder is selected from at least one of iron oxide nickel zinc powder, copper oxide zinc iron powder, cobalt ferrite powder and iron oxide zinc powder.
[0025] By adopting the above technical scheme, ferrite powder has high thermal stability, can maintain chemical properties and structural stability in high temperature environment, and is added to polyurethane cable sheath material. On the one hand, it can serve as a reinforcing material to enhance the toughness of the cable sheath. On the other hand, the ferrite powder is dispersed in the organic polymer matrix material, which can promote the formation of a stable carbon layer when the cable burns, can effectively reduce the burning rate of the material, and also has strong smoke suppression performance.
[0026] In a second aspect, the present application provides a method for preparing the above-mentioned halogen-free flame-retardant polyurethane cable sheath material, comprising the following steps:
[0027] S1, heating and melting thermoplastic polyurethane elastomer, linear low-density polyethylene and ethylene propylene diene rubber, extruding and granulating to obtain pre-crosslinked masterbatch;
[0028] S2, mixing the other raw materials except the cross-linking agent and the pre-cross-linked masterbatch prepared in step S1 in an internal mixer, heating and melting, adding the cross-linking agent for internal mixing, and melt-extruding to obtain an extruded cable sheath;
[0029] S3, cross-linking the extruded cable sheath obtained in step S2 by irradiation with an electron accelerator to obtain a halogen-free flame-retardant polyurethane cable sheath material.
[0030] Furthermore, in step S3, the irradiation dose is 150-270 kGy.
[0031] In summary, the present invention includes at least one of the following beneficial technical effects:
[0032] The present application uses thermoplastic polyurethane elastomer, linear low-density polyethylene and ethylene propylene diene monomer rubber for compounding, and uses them as the base material of the cable sheath. Modified boron nitride nanosheets are introduced into the polyurethane base material, and ferrite powder is used as a synergist to prepare a halogen-free flame-retardant polyurethane cable sheath material. The material has good mechanical strength and toughness, and can reduce the release of toxic smoke while achieving high-efficiency flame retardancy, and can be widely used in various industrial, agricultural and household occasions. DETAILED DESCRIPTION
[0033] The present application designs a halogen-free flame-retardant polyurethane cable sheath material, comprising the following raw materials in parts by weight: 80-110 parts of thermoplastic polyurethane elastomer, 25-38 parts of linear low-density polyethylene, 10-15 parts of ethylene propylene diene rubber, 5-8 parts of compatibilizer, 0.1-1 part of antioxidant, 0.5-1 part of cross-linking agent, and 6-11 parts of filler-type flame retardant; the filler-type flame retardant is modified boron nitride, and the modified boron nitride is prepared by modifying boron nitride nanosheets with sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate.
[0034] The preparation method of the modified boron nitride comprises the following steps:
[0035] 1) Mix boron nitride nanosheets, deionized water and glacial acetic acid, disperse by ultrasonication, add Tris alcohol aqueous solution, heat to 50-65°C, stir to react, cool, filter to obtain the residue, wash with water, and dry to obtain an intermediate material;
[0036] 2) Add an organic solvent into a reaction vessel, add benzoyl peroxide, sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate under nitrogen protection, stir and react for 2-3 hours, add the intermediate material prepared in step 1), stir and react for 2-5 hours, filter, wash the filter residue, and dry to obtain modified boron nitride.
[0037] The halogen-free flame-retardant polyurethane cable sheath material of the present application is prepared by the following method, comprising the following steps:
[0038] S1, heating and melting thermoplastic polyurethane elastomer, linear low-density polyethylene and ethylene propylene diene rubber, extruding and granulating to obtain pre-crosslinked masterbatch;
[0039] S2, mixing the compatibilizer, antioxidant, filler-type flame retardant and the pre-crosslinked masterbatch prepared in step S1 in an internal mixer, heating and melting, adding a crosslinking agent for internal mixing, and melt-extruding to obtain an extruded cable sheath;
[0040] S3, cross-linking the extruded cable sheath obtained in step S2 by irradiation with an electron accelerator to obtain a halogen-free flame-retardant polyurethane cable sheath material.
[0041] The technical problem solved by the present application is that the existing cable sheath prepared based on polyester TPU has poor flame retardant properties as an organic polymer, so the oxygen index (LOI) of polyester TPU without flame retardant treatment is only about 17%, which is far from meeting the fire retardant requirements required for the use of the material, which makes its application site have great fire hazards. The present application uses thermoplastic polyurethane elastomer, linear low-density polyethylene and ethylene propylene rubber for compounding, and uses them as the base material of the cable sheath, introduces modified boron nitride nanosheets into the polyurethane base material, and uses ferrite powder as a synergist to prepare a halogen-free flame retardant polyurethane cable sheath material, which has good mechanical strength and toughness, and reduces the release of toxic smoke while achieving high-efficiency flame retardancy, and can be widely used in various industrial, agricultural and household occasions.
[0042] The present application is further described in detail below in conjunction with specific embodiments.
[0043] Examples 1-5
[0044] Examples 1-5 are halogen-free flame-retardant polyurethane cable sheath materials made from different raw material ratios. The difference lies in the different raw material ratios. The specific raw material ratios in Examples 1-5 are shown in Table 1.
[0045]
[0046] The thermoplastic polyurethane elastomer used in Examples 1-5 is 85A thermoplastic polyurethane elastomer produced by BASF, Germany.
[0047] The compatibilizer used in Examples 1-5 is POE-g-MAH (maleic anhydride grafted octene copolymer), which is N525 POE-g-MAH produced by DuPont Company of the United States.
[0048] The crosslinking agent used in Examples 1-5 was TAIC (triallyl isocyanurate).
[0049] The antioxidant used in Examples 1-5 is phosphite antioxidant Y-213 produced by Good New Materials.
[0050] The filler-type flame retardant in Examples 1-5 is modified boron nitride, and the preparation method comprises the following steps:
[0051] (1) Boron nitride nanosheets, deionized water and glacial acetic acid in a weight ratio of 1:5:0.6 are mixed and ultrasonically dispersed; 20 wt% of Tris alcohol aqueous solution is added, wherein the volume ratio of ethanol to water is 1:1; the temperature is raised to 60°C, stirred for reaction for 3 hours, cooled, filtered to obtain the residue, washed with water, and dried at 60°C to obtain an intermediate material;
[0052] (2) Add an organic solvent to a reaction vessel, raise the temperature to 80°C under nitrogen protection, add benzoyl peroxide, stir for 5 minutes, add sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate, stir and react at 80°C for 3 hours, add the intermediate material prepared in step 1), stir and react for 4 hours, filter, wash the filter residue, and dry to obtain modified boron nitride; wherein the organic solvent is xylene, and the weight ratio of the organic solvent to the intermediate material is 6:1; the amount of the initiator benzoyl peroxide is 2% of the total amount of the sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate.
[0053] Among them, the weight ratio of boron nitride nanosheets, Tris, sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate is 12:30:9:18:30.
[0054] The boron nitride nanosheets used in the preparation process of the modified boron nitride in Examples 1-5 were purchased from Clamart Reagent Company.
[0055] The allyl phosphate used in the preparation process of the modified boron nitride in Examples 1-5 is specifically allyl dimethyl phosphate (CAS: 52628-03-2).
[0056] The method for preparing the sodium lignin sulfonate-maleic anhydride graft copolymer used in the preparation process of the modified boron nitride in Examples 1-5 comprises the following steps:
[0057] Sodium lignin sulfonate was dissolved in distilled water, sodium bisulfite and ammonium persulfate were added, and stirred for 5 minutes to prepare a premixed solution; maleic anhydride and 70wt% ammonia water were mixed in equal weight ratios to prepare an ammoniated mixed solution, and the ammoniated mixed solution was added dropwise to the premixed solution, stirred and reacted at 45°C for 1.5 hours, precipitated with hydrochloric acid, filtered, washed and dried at 45°C to prepare a sodium lignin sulfonate-maleic anhydride graft copolymer. The weight ratio of sodium lignin sulfonate, distilled water, sodium bisulfite, ammonium persulfate and maleic anhydride was 1:5:0.25:0.5:1.
[0058] The preparation method of the halogen-free flame-retardant polyurethane cable sheath material in Examples 1-5 comprises the following steps:
[0059] S1. Thermoplastic polyurethane elastomer, linear low-density polyethylene and ethylene propylene diene monomer rubber are heated and melted at 150°C, extruded and granulated to obtain pre-crosslinked masterbatch; the temperatures of the twin-screw extruder are: 120°C in the feed section, 130°C in the melting section, and 155°C in the die head.
[0060] S2, mixing the compatibilizer, antioxidant, filler-type flame retardant and the pre-crosslinked masterbatch prepared in step S1 in an internal mixer, heating and melting at 190° C., adding a crosslinking agent for internal mixing, and melt-extruding to obtain an extruded cable sheath;
[0061] S3. The extruded cable sheath obtained in step S2 is cross-linked by electron accelerator irradiation to obtain a halogen-free flame-retardant polyurethane cable sheath material; wherein the irradiation dose is set to 200 kGy.
[0062] Example 6
[0063] Example 6 is based on Example 2, except that the compatibilizer used in Example 6 is changed to POP-g-MAH (purchased from Shanghai Pande).
[0064] Example 7
[0065] Example 7 is based on Example 2, except that the propylene phosphate used in the preparation process of modified boron nitride in Example 7 is changed to diethyl isopropylene phosphate (CAS: 5954-28-9).
[0066] Example 8
[0067] Example 8 is based on Example 2, except that the weight ratio of boron nitride nanosheets, Tris, sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate in the raw materials of modified boron nitride in Example 8 is changed to 12:30:15:12:30.
[0068] Example 9
[0069] Example 9 is based on Example 2, except that the weight ratio of boron nitride nanosheets, Tris, sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate in the raw materials of modified boron nitride in Example 9 is changed to 12:30:8:19:30.
[0070] Example 10 is based on Example 2, except that the formula of the halogen-free flame-retardant polyurethane cable sheath material in Example 10 also includes 2 parts by weight of a synergist, the synergist is ferrite powder, and the ferrite powder is zinc iron oxide powder (ZnFe2O4, CAS: 12063-19-3, Sigma-Aldrich Company, Product No. 633844).
[0071] The preparation method of the halogen-free flame-retardant polyurethane cable sheath material in Example 10 comprises the following steps:
[0072] S1. Thermoplastic polyurethane elastomer, linear low-density polyethylene and ethylene propylene diene monomer rubber are heated and melted at 150°C, extruded and granulated to obtain pre-crosslinked masterbatch; the temperatures of the twin-screw extruder are: 120°C in the feed section, 130°C in the melting section, and 155°C in the die head.
[0073] S2, mixing the compatibilizer, antioxidant, filler-type flame retardant, synergist and the pre-crosslinked masterbatch prepared in step S1 in an internal mixer, heating and melting at 190° C., adding a crosslinking agent for internal mixing, and melt-extruding to obtain an extruded cable sheath;
[0074] S3. The extruded cable prepared in step S2 is cross-linked by irradiation with an electron accelerator to prepare a halogen-free flame-retardant polyurethane cable sheath material; wherein the irradiation dose is set to 200 kGy.
[0075] Embodiment 11
[0076] Example 11 is based on Example 2, with the difference that the formula of the halogen-free flame-retardant polyurethane cable sheath material in Example 11 also includes 2.5 parts by weight of a synergist, and the synergist is ferrite powder, and the ferrite powder is iron oxide zinc powder; accordingly, the preparation method of the halogen-free flame-retardant polyurethane cable sheath material in Example 11 refers to Example 10.
[0077] Example 12
[0078] Example 12 is based on Example 2, with the difference that the formula of the halogen-free flame-retardant polyurethane cable sheath material in Example 12 also includes 5 parts by weight of a synergist, the synergist is ferrite powder, and the ferrite powder is iron oxide zinc powder; accordingly, the preparation method of the halogen-free flame-retardant polyurethane cable sheath material in Example 12 refers to Example 10.
[0079] Comparative Example 1
[0080] Comparative Example 1 is based on Example 2, except that: during the preparation process of the modified boron nitride in Comparative Example 1, the reaction process of step (2) is not carried out. Accordingly, the preparation method of the modified boron nitride in Comparative Example 1 becomes:
[0081] Boron nitride nanosheets, deionized water and glacial acetic acid in a weight ratio of 1:5:0.6 are mixed and ultrasonically dispersed; 20wt% of Tris alcohol aqueous solution is added, wherein the volume ratio of ethanol to water is 1:1; the temperature is raised to 60°C, stirred for reaction for 3 hours, cooled, filtered to obtain the residue, washed with water, and dried at 60°C to obtain modified boron nitride; wherein the weight ratio of boron nitride nanosheets to Tris is 12:30.
[0082] Comparative Example 1
[0083] Comparative Example 1 is based on Example 2, except that: during the preparation process of the modified boron nitride in Comparative Example 1, the reaction process of step (2) is not carried out. Accordingly, the preparation method of the modified boron nitride in Comparative Example 1 becomes:
[0084] Boron nitride nanosheets, deionized water and glacial acetic acid in a weight ratio of 1:5:0.6 are mixed and ultrasonically dispersed; 20wt% of Tris alcohol aqueous solution is added, wherein the volume ratio of ethanol to water is 1:1; the temperature is raised to 60°C, stirred for reaction for 3 hours, cooled, filtered to obtain the residue, washed with water, and dried at 60°C to obtain modified boron nitride; wherein the weight ratio of boron nitride nanosheets to Tris is 12:30.
[0085] Comparative Example 2
[0086] Comparative Example 2 is based on Example 2, except that: during the preparation process of the modified boron nitride in Comparative Example 2, the modified boron nitride is not mixed with the alcohol aqueous solution of Tris in step (1). Accordingly, the preparation method of the modified boron nitride in Comparative Example 2 becomes:
[0087] (1) mixing boron nitride nanosheets, deionized water and glacial acetic acid in a weight ratio of 1:5:0.6, and ultrasonically dispersing the mixture; filtering the residue, washing the residue with water, and drying the residue at 60° C. to obtain an intermediate material;
[0088] (2) Add an organic solvent to a reaction vessel, raise the temperature to 80°C under nitrogen protection, add benzoyl peroxide, stir for 5 minutes, add sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate, stir and react at 80°C for 3 hours, add the intermediate material prepared in step 1), stir and react for 4 hours, filter, wash the filter residue, and dry to obtain modified boron nitride; other dosage relationships are the same as in Example 2.
[0089] Comparative Example 3
[0090] Comparative Example 3 is based on Example 2, except that: in the preparation process of the modified boron nitride in Comparative Example 3, benzoyl peroxide is not added in step (2). Accordingly, the preparation method of the modified boron nitride in Comparative Example 3 becomes:
[0091] (1) Mixing boron nitride nanosheets, deionized water and glacial acetic acid in a weight ratio of 1:5:0.6, and ultrasonically dispersing; adding 20 wt % of Tris in an alcohol solution, wherein the volume ratio of ethanol to water is 1:1; heating to 60° C., stirring and reacting for 3 h, cooling, filtering, taking the filter residue, washing with water, and drying at 60° C. to obtain an intermediate material;
[0092] (2) Add an organic solvent to a reaction vessel, raise the temperature to 80°C under nitrogen protection, stir for 5 minutes, add sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate, stir and react at 80°C for 3 hours, add the intermediate material prepared in step 1), stir and react for 4 hours, filter, wash the filter residue, and dry to obtain modified boron nitride; other amounts are the same as in Example 2.
[0093] Comparative Example 4
[0094] Comparative Example 4 is based on Example 2, except that: in the preparation process of the modified boron nitride in Comparative Example 4, dimethylaminoethyl acrylate is not added in step (2). Accordingly, the preparation method of the modified boron nitride in Comparative Example 4 becomes:
[0095] (1) Boron nitride nanosheets, deionized water and glacial acetic acid in a weight ratio of 1:5:0.6 are mixed and ultrasonically dispersed; 20 wt% of Tris alcohol aqueous solution is added, wherein the volume ratio of ethanol to water is 1:1; the temperature is raised to 60°C, stirred for reaction for 3 hours, cooled, filtered to obtain the residue, washed with water, and dried at 60°C to obtain an intermediate material;
[0096] (2) Add an organic solvent to a reaction vessel, raise the temperature to 80°C under nitrogen protection, add benzoyl peroxide, stir for 5 minutes, add sodium lignin sulfonate-maleic anhydride graft copolymer and propylene phosphate, stir and react at 80°C for 3 hours, add the intermediate material prepared in step 1), stir and react for 4 hours, filter, wash the filter residue, and dry to obtain modified boron nitride; wherein the weight ratio of boron nitride nanosheets, Tris, sodium lignin sulfonate-maleic anhydride graft copolymer and propylene phosphate is 12:30:10:30; other dosage relationships are the same as in Example 2.
[0097] Performance Testing
[0098] 1. The tensile properties and elongation at break of the halogen-free flame-retardant polyurethane cable sheath materials prepared in Examples 1-12 and Comparative Examples 1-4 were determined with reference to Standard GB / T2951.11-2008.
[0099] 2. The combustion grades of the halogen-free flame-retardant polyurethane cable sheath materials prepared in Examples 1-12 and Comparative Examples 1-4 were determined with reference to standard GB / T2408-2021.
[0100] 3. The limiting oxygen index of the halogen-free flame-retardant polyurethane cable sheath materials prepared in Examples 1-12 and Comparative Examples 1-4 was determined with reference to standard GB / T 2406.2-2009.
[0101] 4. The mineral oil resistance of the halogen-free flame retardant polyurethane cable sheath materials prepared in Examples 1-12 and Comparative Examples 1-4 was determined according to standard GB / T 2951.21-2008. Specifically, the tensile strength retention of the halogen-free flame retardant polyurethane cable sheath materials was determined at 100°C for 168 hours.
[0102] 5. The aging resistance of the halogen-free flame retardant polyurethane cable sheath materials prepared in Examples 1-12 and Comparative Example 1 was determined according to standard GB / T 2951.11-2008. The specific conditions were as follows: the tensile strength retention rate of the halogen-free flame retardant polyurethane cable sheath materials was determined after 168 hours at 110°C.
[0103] 6. The smoke density test and light transmittance test (the light transmittance is required to be not less than 60%) of the halogen-free flame-retardant polyurethane cable sheath materials prepared in Examples 1-12 and Comparative Example 1 were carried out with reference to standard IEC61034.
[0104] The test results are shown in Tables 2 and 3.
[0105]
[0106]
[0107] By analyzing the data in Table 2 and Table 3 and comparing Examples 1-12 with Comparative Examples 1-4, it can be found that after the boron nitride nanosheets are copolymerized and modified using sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate, the flame retardant properties, mechanical strength, anti-dripping properties and smoke suppression properties of the obtained halogen-free flame retardant polyurethane cable sheath material are significantly improved. Therefore, the polyurethane cable sheath material prepared in the present application can be widely used in the flame retardant and smoke suppression functions of various wires.
[0108] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A halogen-free flame-retardant polyurethane cable sheath material, characterized in that: The invention comprises the following raw materials in parts by weight: 80-130 parts of thermoplastic polyurethane elastomer, 25-38 parts of linear low-density polyethylene, 10-15 parts of ethylene propylene diene rubber, 5-8 parts of compatibilizer, 0.1-1 parts of antioxidant, 0.5-1 parts of cross-linking agent, and 6-11 parts of filler-type flame retardant; The filler-type flame retardant is modified boron nitride, which is prepared by modifying boron nitride nanosheets with sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate; The preparation method of the modified boron nitride comprises the following steps: 1) mixing boron nitride nanosheets, deionized water and glacial acetic acid, ultrasonically dispersing, adding Tris alcohol aqueous solution, heating to 50-65° C., stirring for reaction, cooling, filtering to obtain the residue, washing with water, and drying to obtain an intermediate material; 2) adding an organic solvent to a reaction vessel, adding benzoyl peroxide, sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate under nitrogen protection, stirring and reacting for 2-3 hours, adding the intermediate material prepared in step 1), stirring and reacting for 2-5 hours, filtering, washing the filter residue, and drying to obtain modified boron nitride; In the preparation process of the modified boron nitride, the weight ratio of boron nitride nanosheets, Tris, sodium lignin sulfonate-maleic anhydride graft copolymer, dimethylaminoethyl acrylate and propylene phosphate is 10-20:18-32:8-15:12-19:18-32; The propylene phosphate includes one or more of methacrylate alkoxy phosphate, allyl dimethyl phosphate, and diethyl isopropylene phosphate.
2. The halogen-free flame-retardant polyurethane cable sheath material according to claim 1, characterized in that: The compatibilizer is selected from one or more of POE-g-MAH, POP-g-MAH and MAH-g-SBS.
3. The halogen-free flame-retardant polyurethane cable sheath material according to claim 1, characterized in that: The antioxidant includes one or more of hindered phenol antioxidants, aromatic amine antioxidants, and phosphite antioxidants.
4. The halogen-free flame-retardant polyurethane cable sheath material according to claim 1, characterized in that: The raw materials of the halogen-free flame-retardant polyurethane cable sheath material also include 2-5 parts by weight of a synergist, and the synergist is ferrite powder.
5. A method for preparing the halogen-free flame-retardant polyurethane cable sheath material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, heating and melting thermoplastic polyurethane elastomer, linear low-density polyethylene and ethylene propylene diene rubber, extruding and granulating to obtain pre-crosslinked masterbatch; S2, mixing the other raw materials except the cross-linking agent and the pre-cross-linked masterbatch prepared in step S1 in an internal mixer, heating and melting, Add a cross-linking agent for internal mixing and melt extrusion to obtain an extruded cable sheath; S3, irradiating and cross-linking the extruded cable sheath obtained in step S2 to obtain a halogen-free flame-retardant polyurethane cable sheath material.
6. The method for preparing the halogen-free flame-retardant polyurethane cable sheath material according to claim 5, characterized in that: In step S3, the irradiation dose is 150-270 kGy.
Citation Information
Patent Citations
High-temperature-resistant flame-retardant organosilicon elastomer cable material and preparation method thereof
CN111647271A
TPU sheath material for charging cables as well as preparation and application of TPU sheath material
CN112375371A
Flame-retardant cable and preparation method thereof
CN114989525A
Flame-retardant heat-conducting styrene-butadiene rubber composite material and preparation method thereof
CN116554563A
Corrosion-resistant cable outer sheath material
CN116693989A