A kind of improved nylon 66 particle and preparation method thereof
Through the preparation method of improved nylon 66 particles, combined with specific formulas and process processing, the shortcomings of nylon 66 materials in wear resistance, mechanical strength, dimensional stability and water absorption are solved, and the comprehensive performance improvement and cost saving of the material is achieved. .
Patent Information
- Application Number
- CN202410533556.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-04-29
AI Technical Summary
The prior art is difficult to take into account the wear resistance, mechanical strength, dimensional stability and water absorption of nylon 66 materials at the same time, and lacks a modification solution that can perform well in these aspects.
Using a method of preparing improved nylon 66 particles, nylon 66, polydimethylsiloxane, basalt fiber, molybdenum disulfide, polytetrafluoroethylene, molecular sieve powder, metal salt compounds and antioxidants through the formulation. The process and mixing process are carried out in specific steps, and the improved nylon 66 particles are finally obtained through the extrusion granulation process, ensuring their wear resistance, mechanical properties and dimensional stability while reducing water absorption.
The wear resistance, mechanical properties and dimensional stability of the improved nylon 66 particles are improved, while reducing water absorption, suitable for various working conditions, simplifying the process and reducing costs.
Smart Images

Figure BDA0004818813670000061
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials, and in particular to improved nylon 66 particles and a preparation method thereof. Background Art
[0002] Polyhexamethylene adipamide, commonly known as nylon 66, is a thermoplastic resin, generally made by polycondensation of adipic acid and hexamethylenediamine. Nylon 66 has excellent physical and mechanical properties, electrical properties and self-lubricating properties. It is one of the five general engineering plastics and is widely used in automobiles, machinery, medicine and other fields, with good market prospects. Moreover, nylon 66 can form a variety of modified functional products after compounding with other raw materials. Therefore, the modification research of nylon 66 continues to be highly valued by enterprises.
[0003] At present, the hot modification directions of nylon 66 mainly include wear resistance, mechanical strength, dimensional stability and water absorption, among which there are many existing technologies for improving wear resistance and mechanical strength, such as the technologies disclosed in patent application CN102757641A and patent CN103483812B, but there is still a large room for innovation in technologies that can take into account both dimensional stability and water absorption. In order to let a hundred flowers bloom and enrich the market's selectivity, the more different solutions in this direction, the better.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a method for preparing improved nylon 66 particles. The improved nylon 66 particles obtained by the preparation method not only have excellent wear resistance and mechanical properties, but also have lower water absorption and higher dimensional stability.
[0006] The basic concept of the technical solution adopted by the present invention is as follows:
[0007] A method for preparing improved nylon 66 particles comprises the following steps:
[0008] Step 1, preparing raw materials according to the formula: 100 parts of nylon 66, 0.1-0.5 parts of polydimethylsiloxane, 1-10 parts of basalt fiber, 0.5-5 parts of molybdenum disulfide, 3-12 parts of polytetrafluoroethylene, 5-14 parts of molecular sieve powder, 0.1-6 parts of metal salt compounds based on the amount of metal elements contained, and 0.1-1 parts of antioxidants; wherein the metal salt compound is a combination of one or two of an iron salt compound and a copper salt compound or a zinc salt compound;
[0009] Step 2, dissolving a metal salt compound in water to obtain a metal salt compound solution, adding molecular sieve powder and stirring evenly, adjusting the pH to be alkaline until no precipitate continues to precipitate, filtering and collecting the precipitate and calcining it after washing, reducing the obtained calcined product in a reducing gas, and cooling it to obtain material A;
[0010] Step 3, adding water to polytetrafluoroethylene to prepare an emulsion, then adding material A, mixing and stirring, and then separating and drying to obtain material B;
[0011] Step 4, mixing the material B and the remaining raw materials uniformly to obtain a mixture;
[0012] Step 5, extruding and granulating the mixture, and obtaining the modified nylon 66 particles after cooling, pelletizing and drying.
[0013] As an embodiment, the antioxidant is one or a combination of antioxidant 1098, antioxidant 168 and antioxidant 1010.
[0014] Preferably, the antioxidant is a composition of antioxidant 1098, antioxidant 168 and antioxidant 1010 in a mass ratio of 1:1:2.
[0015] As an embodiment, the metal salt compound is a combination of an iron salt compound and a copper salt compound, and the molar ratio of the iron element to the copper element is (1-2):1.
[0016] As an embodiment, the metal salt compound is a combination of an iron salt compound and a zinc salt compound, and the molar ratio of the iron element to the zinc element is (1-2):1.
[0017] As an embodiment, the metal salt compound is a combination of an iron salt compound, a copper salt compound and a zinc salt compound, and the molar ratio of the iron element, the copper element and the zinc element is (1-1.5):1:1.
[0018] As an embodiment, in step 2, sodium hydroxide solution is used to adjust the pH, and the pH is adjusted to ≥9.
[0019] As an embodiment, the reducing gas is CO or H2.
[0020] As an implementation mode, raw materials are prepared according to the formula: 100 parts of nylon 66, 0.2-0.4 parts of polydimethylsiloxane, 3-7 parts of basalt fiber, 1-3 parts of molybdenum disulfide, 5-10 parts of polytetrafluoroethylene, 7-12 parts of molecular sieve powder, 1-6 parts of metal salt compound, and 0.6-0.9 parts of antioxidant.
[0021] As an embodiment, in step 2, the calcination temperature is 150-250° C., and the calcination time is 1-6 hours; the reduction temperature is 850-1100° C., and the reduction time is 1-4 hours.
[0022] As an implementation mode, in step 4, material B and the remaining raw materials are added into a mixing mixer, the stirring speed is controlled to be 900-1200 r / min, the heating temperature is 70-90° C., and the stirring time is 15-70 min.
[0023] As an embodiment, in step 5, the mixed material is input into a twin-screw extruder for extrusion granulation; the screw speed is 140-210 rpm, and the processing temperature during the processing is 200-240°C in the feeding section, 240-260°C in the plasticizing section, 250-270°C in the homogenizing section, and 200-230°C in the die head temperature.
[0024] The present invention provides an improved nylon 66 particle, which is obtained by any one of the above-mentioned preparation methods.
[0025] Compared with the prior art, the present invention has the following advantages:
[0026] 1. The preparation method of the improved nylon 66 particles of the present invention adopts common and easily available formula components, and the final product effect is achieved by the mutual cooperation between the common components, without the need for complicated and special treatment of the components, thus simplifying the process and saving costs. In addition, the steps of the preparation method are commonly used in industrial production, the operation is simple, and it is particularly suitable for industrial production.
[0027] 2. The improved nylon 66 particles obtained by the preparation method of the present invention have excellent wear resistance, mechanical properties, water absorption and dimensional stability, are suitable for application in more working conditions, and economic benefits are expected.
[0028] 3. In the preparation method of the present invention, the metal ions of the metal salt compound are firstly evenly dispersed on the surface and in the gaps of the molecular sieve, and then coordinated with molybdenum disulfide to improve the wear resistance and dimensional stability of the modified nylon 66 particles;
[0029] Then, polytetrafluoroethylene is evenly attached to the surface of the molecular sieve, which is stable and not easy to fall off. This structure cooperates with polydimethylsiloxane and basalt fiber to reduce the water absorption of the modified nylon 66 particles. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention is clearly and completely described below. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The raw materials used in the following examples can all be purchased from the market, and there is no need to be particularly limited to using products of a specific model or manufacturer.
[0032] The nylon 66 used in the following embodiments refers to ordinary unmodified resin PA66, with a melting point of 255-265°C.
[0033] The polytetrafluoroethylene emulsion is a polytetrafluoroethylene aqueous dispersion formed by dispersing a formulated amount of polytetrafluoroethylene in an appropriate amount of water. The amount of water used is not limited to a specific amount, and can be suitable for dispersion and mixing.
[0034] As an example, the size of molybdenum disulfide is 3-8 μm.
[0035] As an example, the size of the molecular sieve powder is 10 to 30 μm.
[0036] The metal salt compound contains 0.1 to 6 parts of metal elements by weight, that is, when 100 parts of nylon 66 are added, the amount of the metal salt compound added satisfies that the amount of metal elements contained therein is 0.1 to 6 parts.
[0037] The metal salt compound is a combination of an iron salt compound and one or two of a copper salt compound and a zinc salt compound, and can be a common iron salt compound and a copper salt compound and a zinc salt compound on the market, and is not limited to salts of specific anions.
[0038] The molecular sieve may be commercially available 2A, 3A, 4A, 5A, ZSM-8, ZSM-11, Silicalite-1, SAPO-34, AlPO4-5, AlPO-18 or TS-1.
[0039] Example 1
[0040] A method for preparing improved nylon 66 particles comprises the following steps:
[0041] Step 1, preparing raw materials according to the formula: 100 parts of nylon 66, 0.1 parts of polydimethylsiloxane, 10 parts of basalt fiber, 5 parts of molybdenum disulfide, 3 parts of polytetrafluoroethylene, 14 parts of 5A molecular sieve powder, 0.1 parts of metal salt compounds based on the amount of metal elements contained, and 0.1 parts of antioxidant 1098; wherein the metal salt compounds are iron salt compounds and copper salt compounds, and the molar ratio of iron element to copper element is 2:1;
[0042] Step 2, dissolving the metal salt compound in water to obtain a metal salt compound solution, adding molecular sieve powder and stirring evenly, adjusting the pH to ≥ 9 with sodium hydroxide solution until no precipitate continues to precipitate, filtering, collecting the precipitate and calcining it after washing, the calcination temperature is 150° C., and the calcination time is 6 hours; the obtained calcined product is reduced in H2 gas, the reduction temperature is 850° C., the reduction time is 4 hours, and material A is obtained after cooling;
[0043] Step 3, adding water to polytetrafluoroethylene to prepare an emulsion, then adding material A, mixing and stirring, and then separating and drying to obtain material B;
[0044] Step 4, adding the material B and the remaining raw materials into a mixing mixer and mixing them evenly, controlling the stirring speed to 900 r / min, the heating temperature to 70° C., and the stirring time to 15 min to obtain a mixture;
[0045] Step 5, input the mixed material into a twin-screw extruder for extrusion granulation, the screw speed is 140rpm, the processing temperature during the processing is 200°C in the feeding section, 240°C in the plasticizing section, 250°C in the homogenizing section, and 200°C in the die head temperature; then after cooling, pelletizing and drying, the improved nylon 66 particles are obtained.
[0046] Example 2
[0047] A method for preparing improved nylon 66 particles comprises the following steps:
[0048] Step 1, preparing raw materials according to the formula: 100 parts of nylon 66, 0.5 parts of polydimethylsiloxane, 1 part of basalt fiber, 0.5 parts of molybdenum disulfide, 12 parts of polytetrafluoroethylene, 5 parts of ZSM-11 molecular sieve powder, 6 parts of metal salt compounds based on the amount of metal elements contained, and 1 part of antioxidant 168; wherein the metal salt compounds are iron salt compounds and zinc salt compounds, and the molar ratio of iron element to zinc element is 1:1;
[0049] Step 2, dissolving the metal salt compound in water to obtain a metal salt compound solution, adding molecular sieve powder and stirring evenly, adjusting the pH to ≥ 9 with sodium hydroxide solution until no precipitate continues to precipitate, filtering, collecting the precipitate and calcining it after washing, the calcination temperature is 250° C., and the calcination time is 1 h; the obtained calcined product is reduced in H2 gas, the reduction temperature is 1100° C., the reduction time is 1 h, and material A is obtained after cooling;
[0050] Step 3, adding water to polytetrafluoroethylene to prepare an emulsion, then adding material A, mixing and stirring, and then separating and drying to obtain material B;
[0051] Step 4, adding the material B and the remaining raw materials into a mixer and mixing them evenly, controlling the stirring speed to 1200 r / min, the heating temperature to 90° C., and the stirring time to 70 min to obtain a mixture;
[0052] Step 5, inputting the mixed material into a twin-screw extruder for extrusion granulation, the screw speed is 210rpm, the processing temperature during the processing is 240°C in the feeding section, 260°C in the plasticizing section, 270°C in the homogenizing section, and 230°C in the die head; then after cooling, pelletizing and drying, the improved nylon 66 particles are obtained.
[0053] Example 3
[0054] The difference from Example 1 is that the raw materials are prepared according to the formula: 100 parts of nylon 66, 0.2 parts of polydimethylsiloxane, 3 parts of basalt fiber, 1 part of molybdenum disulfide, 5 parts of polytetrafluoroethylene, 7 parts of molecular sieve powder, 1 part of metal salt compound based on the metal element contained, and 0.6 parts of antioxidant. The rest are the same as Example 1.
[0055] Example 4
[0056] The difference from Example 2 is that the raw materials are prepared according to the formula: 100 parts of nylon 66, 0.4 parts of polydimethylsiloxane, 7 parts of basalt fiber, 3 parts of molybdenum disulfide, 10 parts of polytetrafluoroethylene, 12 parts of molecular sieve powder, 6 parts of metal salt compound based on the metal element contained, and 0.9 parts of antioxidant. The rest are consistent with Example 2.
[0057] Example 5
[0058] The difference from Example 1 is that the antioxidant is a composition of antioxidant 1098, antioxidant 168 and antioxidant 1010 in a mass ratio of 1:1:2, and the other ingredients remain unchanged.
[0059] Example 6
[0060] The difference from Example 1 is that the metal salt compound is a combination of an iron salt compound, a copper salt compound and a zinc salt compound, the molar ratio of the iron element, the copper element and the zinc element is 1.5:1:1, and the others remain unchanged. And the specific iron salt compound and the copper salt compound used are the same as those in Example 1.
[0061] Comparative Example 1
[0062] The difference from Example 1 is that polytetrafluoroethylene is missing from the raw material formula, and the corresponding processing steps 3 and 4 are also omitted, and material A is directly mixed with the remaining components to obtain a mixed material and then granulated. The rest is the same as Example 1.
[0063] Comparative Example 2
[0064] The difference from Example 1 is that the raw material formula only lacks polydimethylsiloxane, and the rest is consistent with Example 1.
[0065] Comparative Example 3
[0066] The difference from Example 1 is that all the raw material formulas are directly stirred together to obtain a mixture, which is then granulated. The granulation process is the same as that of Example 1.
[0067] Test example
[0068] The test samples are nylon 66 products of Examples 1-6 and Comparative Examples 1-3. The test performance and results are shown in Table 1. Examples 1-6 in Table 1 are Examples 1-6 of the present invention, and Comparative Examples 1-3 are Comparative Examples 1-3.
[0069] When testing the water absorption, the pellets obtained in Examples 1-6 and Comparative Examples 1-3 were placed in a vacuum oven at 100°C and dried for 8 hours, and then injection molded at 265°C to prepare samples with a sample size of 60 mm×60 mm×2 mm. The injection molded samples were dried at 50°C for 96 hours, weighed after cooling, and then immersed in distilled water at 23°C for 24 hours to measure the water absorption mass fraction.
[0070] Table 1
[0071]
[0072] It can be seen from the test data in Table 1 that the tensile strength, flexural strength and modulus, wear resistance and dimensional stability of the improved nylon 66 particles prepared by Examples 1-6 of the present invention are improved to varying degrees, and the water absorption is low. The comprehensive performance of the material is excellent and the market prospect is good.
[0073] However, the products of Comparative Examples 1-3 did not adopt the technical solution of the present invention, and the performance differences were significant.
[0074] Although the embodiments disclosed in the present invention are as above, the contents described are only embodiments adopted to facilitate understanding of the present invention and are not intended to limit the present invention. Any technician in the field to which the present invention belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in the present invention, but the patent protection scope of the present invention shall still be subject to the scope defined in the attached claims.
Claims
1. A method for preparing improved nylon 66 particles, characterized in that: The following steps are involved: Step 1, preparing raw materials according to the formula: 100 parts of nylon 66, 0.1-0.5 parts of polydimethylsiloxane, 1-10 parts of basalt fiber, 0.5-5 parts of molybdenum disulfide, 3-12 parts of polytetrafluoroethylene, 5-14 parts of molecular sieve powder, 0.1-6 parts of metal salt compounds based on the amount of metal elements contained, and 0.1-1 parts of antioxidants; wherein the metal salt compound is a combination of one or two of an iron salt compound and a copper salt compound or a zinc salt compound; Step 2, dissolving a metal salt compound in water to obtain a metal salt compound solution, adding molecular sieve powder and stirring evenly, adjusting the pH to be alkaline until no precipitate continues to precipitate, filtering and collecting the precipitate and calcining it after washing, reducing the obtained calcined product in a reducing gas, and cooling it to obtain material A; Step 3, adding water to polytetrafluoroethylene to prepare an emulsion, then adding material A, mixing and stirring, and then separating and drying to obtain material B; Step 4, mixing the material B and the remaining raw materials uniformly to obtain a mixture; Step 5, extruding and granulating the mixture, cooling, pelletizing and drying to obtain the improved nylon 66 particles; The metal salt compound is a combination of an iron salt compound and a copper salt compound, and the molar ratio of the iron element to the copper element is (1-2):1; or, the metal salt compound is a combination of an iron salt compound and a zinc salt compound, and the molar ratio of the iron element to the zinc element is (1-2):1; or, the metal salt compound is a combination of an iron salt compound, a copper salt compound and a zinc salt compound, and the molar ratio of the iron element, the copper element and the zinc element is (1-1.5):1:1; In step 2, the reducing gas is CO or H2; the calcination temperature is 150-250°C, and the calcination time is 1-6 hours; the reduction temperature is 850-1100°C, and the reduction time is 1-4 hours.
2. The method for preparing improved nylon 66 particles according to claim 1, characterized in that: The antioxidant is one or a combination of antioxidant 1098, antioxidant 168 and antioxidant 1010.
3. The method for preparing improved nylon 66 particles according to claim 2, characterized in that: The antioxidant is a composition of antioxidant 1098, antioxidant 168 and antioxidant 1010 in a mass ratio of 1:1:
2.
4. The method for preparing improved nylon 66 particles according to claim 1, characterized in that: In step 2, sodium hydroxide solution is used to adjust the pH, and the pH is adjusted to ≥9.
5. The method for preparing improved nylon 66 particles according to claim 1, characterized in that: Prepare the raw materials according to the formula: 100 parts of nylon 66, 0.2-0.4 parts of polydimethylsiloxane, 3-7 parts of basalt fiber, 1-3 parts of molybdenum disulfide, 5-10 parts of polytetrafluoroethylene, 7-12 parts of molecular sieve powder, 1-6 parts of metal salt compound, and 0.6-0.9 parts of antioxidant.
6. The method for preparing improved nylon 66 particles according to claim 1, characterized in that: In the step 4, material B and the remaining raw materials are added into a mixing mixer, the stirring speed is controlled to be 900-1200 r / min, the heating temperature is 70-90° C., and the stirring time is 15-70 min.
7. The method for preparing improved nylon 66 particles according to claim 1, characterized in that: In step 5, the mixed material is input into a twin-screw extruder for extrusion granulation; the screw speed is 140-210 rpm, and the processing temperature during the processing is 200-240°C in the feeding section, 240-260°C in the plasticizing section, 250-270°C in the homogenizing section, and 200-230°C in the die head.
8. A modified nylon 66 particle, characterized in that: Obtained according to the preparation method according to any one of claims 1 to 7.
Citation Information
Patent Citations
High toughness and wear resistant nylon and preparation method thereof
CN102757641A
A method for preparing abrasion-resistant nylon 66 containing antioxidants
CN103483812B
Modified wear-resistant nylon as well as preparation method and application
CN110452529A
Modified nylon 66 particle and preparation method thereof
CN115537021A