A method for photocatalytic degradation of Sudan red

By adding alkyl glycosides to Sudan Red aqueous solution and using Ag@Ag2O/AgCl photocatalytic material, photocatalyzing is solved by using sunlight to produce toxic substances caused by Sudan Red water insolubleness and traditional treatment methods, achieving high efficiency and low cost degradation effect.

CN118307087BActive Publication Date: 2024-11-15JIANGSU POLYTECHNIC COLLEGE OF AGRI & FORESTRY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410552480.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-07
Publication Date
2024-11-15
Estimated Expiration
2044-05-07

AI Technical Summary

Technical Problem

The prior art has water insoluble problems when dealing with Sudan Red, which leads to the production of intermediate poisons in traditional microbial treatment, high electrochemical treatment costs, photocatalytic materials are dependent on ultraviolet light and have low efficiency, making it difficult to effectively degrade Sudan Red.

Method used

Using alkyl glycosides (APG or AEG) as dispersant and co-solvent, Sudan Red is converted into aqueous solution, and Ag@Ag2O/AgCl is used as photocatalytic material to perform photocatalytic degradation through sunlight, and use visible light and solar energy to improve degradation efficiency .

Benefits of technology

It achieves efficient degradation of Sudan Red, avoids the generation of toxic substances, reduces costs and energy consumption, expands the application range, and is simple to prepare the materials, safe and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118307087B_ABST
    Figure CN118307087B_ABST
Patent Text Reader

Abstract

The invention discloses a method for photocatalytic degradation of Sudan red, the method comprising the following steps: adding glycoside compounds to an aqueous suspension containing Sudan red, after ultrasonic treatment, heating in a water bath to obtain a Sudan red aqueous solution; adding photocatalytic material Ag@Ag2O / AgCl, stirring in the dark until the suspension is adsorbed and desorbed in equilibrium, and then placing the suspension under sunlight for irradiation, and continuously stirring during the irradiation process until Sudan red is completely degraded. The present invention prepares Sudan red aqueous solution by adding glycoside compounds, and the used glycoside compounds have complete biodegradability, safety and environmental protection, and no toxic substances are produced; the obtained Sudan red aqueous solution uses sunlight resources for photocatalytic degradation, and the process is simple, the reaction conditions are warm, and energy saving and consumption reduction are reduced; the photocatalytic material preparation method used is simple, integrating adsorption and photocatalysis, and Sudan red can be completely degraded in the end, effectively solving the problem that fat-soluble dyes are insoluble in water and produce toxic substances during degradation, and the application range is wider.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for photocatalytic degradation of Sudan red, belonging to the technical field of harmful substance degradation. Background Art

[0002] Sudan, also known as oil-soluble red or solvent red, is a synthetic lipophilic azo compound. Sudan II, III, and IV are all derivatives of Sudan I (SD I, also known as 1-phenylazo-2-naphthol). Sudan series dyes are generally insoluble in water but easily soluble in organic solvents. They are often used in industrial products such as solvents, gasoline, motor oil, shoe polish, and car wax, as well as cell coloring in biochemical toxicology research. They can also be used to color fireworks. They are all industrial dyes. SD I and its metabolites can form adducts with animal DNA and are potential carcinogens. They can cause tumors in organs such as the bladder, spleen, and liver. In addition, Sudan is also allergenic to the skin and can cause dermatitis in humans. During the use of Sudan series dyes, a considerable amount will inevitably be discharged into the sewage treatment system or directly into the natural environment, which not only affects the water quality, but may also affect the health of organisms and humans through the food chain.

[0003] At present, the degradation methods of Sudan red mainly include photocatalytic degradation, microbial degradation, electrochemical treatment technology, etc. Sudan red is insoluble in water. Traditional microbial treatment technology has certain limitations in treating Sudan red. It will produce intermediate product aniline, which is still toxic, harmful to the environment, and can cause pollution to water bodies. Electrochemical treatment has high cost and is difficult to apply in practice. At present, most of the materials used for photocatalytic treatment of wastewater are nano-TiO2, which can only use ultraviolet light, with low light energy utilization rate, and often treat water-soluble wastewater. Sudan red is insoluble in water. Under certain conditions, Sudan red wastewater is easy to form precipitation and difficult to be used by other organisms, thus producing toxic effects. Under general experimental conditions, NaCl anhydrous ethanol is often used as simulated wastewater, or acetonitrile is used as solvent, and SDⅠ acetonitrile solution is mixed with distilled water to obtain SDⅠ aqueous solution; some directly use ultrasonic treatment to form suspended particles, which are then filtered for catalytic degradation. These methods are easy to implement under experimental conditions, but cannot be effectively applied in practice and are costly. Effectively solving the solubility problem of Sudan red in water systems can be beneficial to photocatalytic degradation.

[0004] Alkyl polyglycoside (APG) is a non-ionic surfactant that contains a hydrophilic sugar structure and a hydrophobic alkyl fatty chain. Since the raw materials for the synthesis of APG are sugars and fatty alcohols, it has become a new generation of green surfactants recognized worldwide. It is non-toxic, non-irritating, and completely biodegradable. The degradation products are CO2, water and inorganic elements, which are environmentally friendly. APG is widely used in the pharmaceutical, detergent, food, and cosmetics industries. In addition, it has broad application prospects in catalysis, adsorption, nanotechnology, separation analysis, biotechnology, agriculture, and environmental governance. Summary of the invention

[0005] Purpose of the invention: The purpose of the present invention is to provide a green and environmentally friendly method for photocatalytic degradation of Sudan red.

[0006] Technical solution: The method for photocatalytic degradation of Sudan red of the present invention comprises the following steps: adding glycoside compounds to an aqueous suspension containing Sudan red, heating in a water bath to obtain an aqueous solution of Sudan red; adding photocatalytic material Ag@Ag2O / AgCl, stirring in the dark until the suspension reaches adsorption-desorption equilibrium, and then placing the suspension under sunlight for irradiation, and continuously stirring during the irradiation process until the Sudan red is completely degraded.

[0007] Wherein, the glycoside compound includes APG or AEG.

[0008] Wherein, the volume of the added glycoside compound stock solution is 6-7 mL.

[0009] The invention also includes a method for preparing a Sudan red aqueous suspension, which specifically comprises: adding Sudan red into water, and subjecting the water suspension to ultrasonic treatment to obtain the Sudan red aqueous suspension.

[0010] Wherein, the Sudan Red includes one or more of Sudan Red I, II, III and IV.

[0011] Among them, the solid-liquid ratio of water, Sudan red and glycoside compounds is 0.8~1 L: 0.008~0.012 g: 6~7mL.

[0012] The water bath heating condition is 80-100° C. and the heating time is 25-35 min.

[0013] The preparation of the photocatalytic material Ag@Ag2O / AgCl includes the following steps: adding hexadecyltrimethylammonium bromide to sodium alginate and ultrasonically dispersing it; adding high specific surface area graphene oxide (GO) and ultrasonically dispersing it; dropping AgNO3 solution under stirring conditions; dropping Ca(NO3)2 solution, NaCl solution and KOH solution under stirring conditions, standing, taking small particle precipitates and adding deionized water, placing them under a xenon lamp light source under stirring conditions, washing with deionized water, centrifuging, and vacuum freeze-drying to obtain the photocatalytic material Ag@Ag2O / AgCl.

[0014] The volume ratio of the sodium alginate solution, the hexadecyltrimethylammonium bromide solution and the graphene oxide is 6-8:1:1-3; the concentrations of the sodium alginate, the hexadecyltrimethylammonium bromide and the graphene oxide are 4 g / L, 10 g / L and 2 g / L respectively.

[0015] Among them, the volume ratio of the AgNO3, Ca(NO3)2, NaCl and KOH solutions is 2-3:10:1-2:6; the concentrations of the AgNO3, Ca(NO3)2, NaCl and KOH solutions are 50g / L, 30g / L, 10g / L and 10g / L respectively.

[0016] Wherein, after adding the photocatalytic material Ag@Ag2O / AgCl, the method further comprises a step of adjusting the pH to 3.0-5.0.

[0017] Wherein, the stirring condition in the dark is to control the temperature at 30-50°C.

[0018] The suspension is placed under sunlight for irradiation during a period of time when the solar radiation energy changes the least on a sunny day, that is, between 11:00 and 13:00 every day.

[0019] The mechanism of photocatalytic material degradation is as follows: under visible light irradiation, Ag2O and AgCl are excited to generate corresponding photogenerated holes h + Heguangsheng Electronics - They are located in the valence band and conduction band respectively. The photogenerated electrons are captured by Ag due to the SPR effect and transferred to the surface of the material, and then captured by O2 in the solution to form active oxygen groups·O2 - , thereby decomposing SDI and inhibiting the recombination of photogenerated carriers. Holes in the valence band will react with H2O and OH outside the material. - React to generate ·OH, these active groups (h + 、O2 - , ·OH) has strong oxidizing properties, which enhances the photocatalytic performance of the composite material. In addition, the holes on the surface of AgCl particles h + , and can also be used with Cl− The reaction generates Cl 0 , Cl 0 The oxidation ability is strong, which can quickly oxidize the SDI molecules adsorbed on the catalyst surface. 0 It is reduced to Cl − , thus effectively ensuring the stability of the catalytic system. The addition of GO to the photocatalytic material can effectively capture the e- − , inhibiting the recombination of photogenerated electrons and holes, improving the charge separation efficiency, and promoting the improvement of the photocatalytic performance of the composite material.

[0020] Beneficial effects: Compared with the prior art, the present invention has the following outstanding and significant advantages: the Sudan red photocatalytic degradation method of the present invention, by adding a small amount of glycoside compounds (APG or AEG) as dispersants and co-solvents to prepare Sudan red aqueous solution through high-temperature dissolution, the APG or AEG used is completely biodegradable, safe, environmentally friendly, cheap, and does not produce toxic substances; the Sudan red aqueous solution obtained uses sunlight resources for photocatalytic degradation, the process is simple, no harsh conditions are required, the reaction conditions are warm, and energy saving and consumption reduction are achieved; the photocatalytic material Ag@Ag2O / AgCl used has a simple preparation method, strong adsorption capacity, reduces a single adsorption effect, integrates adsorption and photocatalysis, and can finally degrade Sudan red, effectively solving the problem that fat-soluble dyes are insoluble in water and that toxic substances are produced during the degradation process, and has a wider range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 UV-visible absorption spectrum of SDⅠAPG in aqueous solution;

[0022] Figure 2 SEM images of photocatalytic materials;

[0023] Figure 3 Energy spectrum of photocatalytic materials;

[0024] Figure 4 Elemental distribution map of photocatalytic materials;

[0025] Figure 5 XRD patterns of photocatalytic materials;

[0026] Figure 6 The concentration is 10mg•L -1 UV-Vis absorption spectrum of SDⅠAPG aqueous solution degradation (Ag@Ag2O / AgCl);

[0027] Figure 7 The concentration is 8mg•L -1 UV-Vis absorption spectrum of SDⅠAPG aqueous solution degradation (Ag@Ag2O / AgCl);

[0028] Figure 8 The concentration is 6mg•L -1 UV-Vis absorption spectrum of SDⅠAPG aqueous solution degradation (Ag@Ag2O / AgCl);

[0029] Fig. 9 The concentration is 5mg•L -1 UV-Vis absorption spectrum of SDⅠAEG aqueous solution degradation (Ag@Ag2O / AgCl);

[0030] Fig.10 The concentration is 5mg•L -1 UV-Vis absorption spectrum of SDⅠAEG aqueous solution degradation (TiO2);

[0031] Fig.11 The concentration is 5mg•L -1 UV-Vis absorption spectrum of SDⅠAEG aqueous solution degradation (Ag@AgCl / CA). DETAILED DESCRIPTION

[0032] The technical solution of the present invention is further described below in conjunction with the accompanying drawings. Example

[0033] Take 0.010g SDⅠ (Shanghai Yuanye Biotechnology Co., Ltd.) and add it to a 1000mL beaker, and add 1000mL 80℃ hot water, stir with a glass rod after mixing, place it in an ultrasonic cleaner, and ultrasonically treat it for 30min at a temperature of 80℃ and a power of 60W. Then add 7mL of APG stock solution (alkyl glycoside 0810, Jiangsu Wanqi Biotechnology Co., Ltd., neutral, solid content ≧50%), place it in a 100℃ water bath and heat to dissolve, stir with a glass rod intermittently, and control the time to be 30min to prepare an APG aqueous solution of SDⅠ.

[0034] UV-Vis absorption spectrum Figure 1 As shown in the figure, Sudan red was suspended in water and after ultrasonic treatment, SDⅠ had no obvious absorption peak (red line), which was caused by SDⅠ being suspended in water without dissolving. The APG aqueous solution of SDⅠ (blue line) formed after adding 7mL of APG stock solution showed characteristic absorption peaks at 305 and 484nm, respectively, of which 305nm was a weak absorption peak, which was the absorption peak produced by the transition of naphthalene ring n→σ* in the near-ultraviolet region. The characteristic peak of 484nm in the visible region was a strong broad absorption peak of the azo conjugated system of SDⅠ in the visible light region, and a weak shoulder peak appeared at 423nm in the visible region. Example

[0035] Take 100mL of 4 g / L sodium alginate (SA) solution, add 16mL of 10g / L hexadecyltrimethylammonium bromide (CTAB) surfactant, and ultrasonically disperse for 30min. Then add 20mL of 2g / L graphene oxide (GO, Shanghai Maoguo Nano Technology Co., Ltd.) dispersion, and ultrasonically disperse for 15min to fully mix the GO dispersion with the SA solution. Under magnetic stirring, slowly add 12mL of 50g / L AgNO3 solution to the mixed solution. After the addition is completed, continue magnetic stirring for 15min, then slowly add 40mL of Ca(NO3)2 solution (concentration 30g / L), 12mL of NaCl solution (concentration 10g / L) and 24mL of KOH (concentration 10g / L) solution to the mixed solution, magnetically stir for 30min and let stand for 24h. The small particle precipitate obtained above was added to a 250mL conical flask, and 50 mL of deionized water was added. Under magnetic stirring, it was placed under a 350W xenon light source for 1 hour. It was washed with deionized water for 5-6 times, and then prepared into a 400mL small particle suspension containing the photocatalytic material Ag@Ag2O / AgCl with deionized water. Part of the suspension was taken, centrifuged, and vacuum freeze-dried to obtain the Ag@Ag2O / AgCl photocatalytic material for detection.

[0036] Figure 2 The material morphology observed by high-resolution field emission scanning electron microscopy (SEM) is shown in Figure 2. A large number of irregularly shaped nano-Ag2O and AgCl particles are loaded on the folded structure of the catalytic material, which also loads a certain amount of nano-silver particles. These particles overlap and accumulate in clusters, and the particle size is uneven. It can be seen that the Ag@Ag2O / AgCl particles are successfully loaded on the Ca 2+ The cross-linked GO / CA wrinkles are conducive to the adsorption and rapid degradation of dyes by the composite material, effectively improving the photocatalytic performance of the composite material.

[0037] Figure 3 and Figure 4 They are the EDS spectrum and elemental analysis of the catalytic material. The sample contains Ag, Cl, C, O, Ca, Br and other elements, among which the mass concentration of Ag element is relatively large, second only to C element, and the concentration of Ag atoms is also relatively large, second only to C and O. The concentration of Cl atoms is about 1 / 3 of that of Ag atoms, that is, Ag(O):AgCl=2:1, indicating that in addition to AgCl, the composite material also contains nano-Ag2O particles and Ag particles.

[0038] Take the photocatalytic material for X-ray diffraction (XRD), Figure 5 The XRD spectrum of the photocatalytic material is shown in Figure 2 θThe five characteristic diffraction peaks at angles of 27.7°, 32.2°, 46.2°, 54.9° and 57.6° are respectively attributed to the (111), (200), (220), (311) and (222) crystal planes of nano-AgCl; θ The four characteristic diffraction peaks at angles of 31.6°, 38.2°, 56.2° and 65.9° are respectively attributed to the (111), (200), (220) and (311) crystal planes of nano-Ag2O; θ The two characteristic diffraction peaks at angles of 38.2° and 45.2° are attributed to the (111) and (200) crystal planes of nano-Ag, respectively. Example

[0039] Take 10 mL of the Ag@Ag2O / AgCl suspension prepared in Example 2, centrifuge to obtain Ag@Ag2O / AgCl particles, and then mix with 100 mL of SDⅠ with a concentration of 10 mg·L -1 After mixing with the APG aqueous solution, add it into a 100 mL Erlenmeyer flask, adjust the initial pH value to 4.0, control the temperature at 20 °C, stir in the dark for 30 min, and then directly irradiate the suspension after adsorption equilibrium under sunlight between 11:00 and 13:00 on a sunny day for 60 min, and stir it with a magnetic stirrer during the photocatalytic reaction.

[0040] Figure 6 It shows that after dark adsorption, the adsorption rate is 27.40%, and after photocatalysis, it is completely degraded after 60 minutes, and the removal rate reaches 100%. Example

[0041] Take 10 mL of the Ag@Ag2O / AgCl suspension prepared in Example 2, centrifuge to obtain Ag@Ag2O / AgCl particles, and then mix with 100 mL of SDⅠ with a concentration of 8 mg·L -1 After mixing with the APG aqueous solution, add it into a 100mL Erlenmeyer flask, adjust the initial pH value to 4.0, control the temperature at 30℃, stir in the dark for 30 min, and then directly irradiate the suspension after adsorption equilibrium under sunlight between 11:00-13:00 on a sunny day for 30 min, and stir with a magnetic stirrer during the photocatalytic reaction.

[0042] Figure 7 It shows that after dark adsorption, the adsorption rate is 55.22%, and after photocatalysis, it is almost completely degraded after 30 minutes, with a removal rate of 98%. Example

[0043] Take 10 mL of the Ag@Ag2O / AgCl suspension prepared in Example 2, centrifuge to obtain Ag@Ag2O / AgCl particles, and then mix with 100 mL of SDⅠ with a concentration of 6 mg·L -1 After mixing with the APG aqueous solution, add it into a 100mL Erlenmeyer flask, adjust the initial pH value to 4.0, control the temperature at 40℃, stir in the dark for 30 min, and then directly irradiate the suspension after adsorption equilibrium under sunlight between 11:00-13:00 on a sunny day for 20 min, and stir with a magnetic stirrer during the photocatalytic reaction.

[0044] Figure 8 It shows that after dark adsorption, the adsorption rate is 60.40%, and after photocatalysis, it is almost completely degraded after 20 minutes, with a removal rate of 99%. Example

[0045] Take 10 mL of the Ag@Ag2O / AgCl suspension prepared in Example 2, centrifuge to obtain Ag@Ag2O / AgCl particles, and then mix with 100 mL of SDⅠ with a concentration of 5 mg·L -1 After mixing with the AEG aqueous solution, add it into a 100mL Erlenmeyer flask, adjust the initial pH value to 4.0, control the temperature at 30℃, stir in the dark for 30 min, and then directly irradiate the suspension after adsorption equilibrium under sunlight between 11:00-13:00 on a sunny day for 10 min, and stir with a magnetic stirrer during the photocatalytic reaction.

[0046] Fig. 9 It shows that after dark adsorption, the adsorption rate is 80.70%, and after photocatalysis, it is completely degraded after 10 minutes, with a removal rate of 100%.

[0047] Comparative Example 1

[0048] Referring to the method of Example 6, 100 mL of SDⅠ with a concentration of 5 mg·L -1 AEG aqueous solution, nano-TiO2 and Ag@AgCl / CA prepared in the literature (preparation process reference ZL202210850837.X) were selected as photocatalytic comparison materials, and catalytic degradation was carried out using sunlight. The results are shown in Table 1. Fig.10 and Fig.11 The results show that the AEG aqueous solution prepared by the present invention can be completely degraded under sunlight, but the prepared photocatalytic material has stronger adsorption capacity, higher light energy utilization and shorter degradation time than nano-TiO2 and Ag@AgCl / CA.

[0049] Table 1 Effects of different photocatalytic materials on the adsorption and degradation of SDⅠ

[0050] Material Adsorption capacity Light energy utilization Degradation time / min <![CDATA[Nano-TiO2]]> 35% Ultraviolet light in sunlight 60 Ag@AgCl / CA 44% Visible and ultraviolet light in sunlight 25 Photocatalytic materials prepared by this patent 80% Visible and ultraviolet light in sunlight 10

[0051] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for photocatalytic degradation of Sudan red, It is characterized in that The following steps are involved: Add glycoside compounds to the water suspension containing Sudan red, heat it in a water bath, and obtain Sudan red aqueous solution; add photocatalytic material Ag@Ag 2 O / AgCl, stirring in the dark until the suspension is in adsorption-desorption equilibrium, and then placing the suspension under sunlight for irradiation, stirring continuously during the irradiation process until Sudan red is completely degraded; The glycoside compound includes alkyl glycoside or alcohol ether glycoside; The photocatalytic material Ag@Ag 2 The preparation of O / AgCl comprises the following steps: adding hexadecyltrimethylammonium bromide solution to sodium alginate solution, ultrasonically dispersing, adding graphene oxide, and ultrasonically dispersing; AgNO was added dropwise under stirring 3 solution; add Ca(NO 3 ) 2 The solution, NaCl solution and KOH solution were allowed to stand, and small precipitates were added to deionized water, and irradiated under a xenon light source under stirring conditions, washed with deionized water, centrifuged, and vacuum freeze-dried to obtain the photocatalytic material Ag@Ag 2 O / AgCl.

2. The method for photocatalytic degradation of Sudan Red according to claim 1, It is characterized in that The Sudan Red includes one or more of Sudan Red I, Sudan Red II, Sudan Red III and Sudan Red IV.

3. The method for photocatalytic degradation of Sudan Red according to claim 1, It is characterized in that The water bath heating condition is 80-100° C. and the heating time is 25-35 min.

4. The method for photocatalytic degradation of Sudan Red according to claim 1, It is characterized in that The volume ratio of the sodium alginate solution, the hexadecyltrimethylammonium bromide solution and the graphene oxide is 6-8:1:1-3; the concentrations of the sodium alginate, the hexadecyltrimethylammonium bromide and the graphene oxide are 4 g / L, 10 g / L and 2 g / L respectively.

5. The method for photocatalytic degradation of Sudan Red according to claim 1, It is characterized in that The AgNO 3 Solution, Ca(NO 3 ) 2 The volume ratio of the solution, the NaCl solution and the KOH solution is 2-3:10:1-2:6; the AgNO 3 Solution, Ca(NO 3 ) 2 The concentrations of the solution, NaCl solution, and KOH solution are 50 g / L, 30 g / L, 10 g / L, and 10 g / L, respectively.

6. The method for photocatalytic degradation of Sudan Red according to claim 1, It is characterized in that The addition of photocatalytic material Ag@Ag 2 The step of adjusting pH is also included after O / AgCl, and the pH is adjusted to 3.0-5.

0.

7. The method for photocatalytic degradation of Sudan Red according to claim 1, It is characterized in that The stirring condition in the dark is to control the temperature at 30-50°C.