Sulfonate modified basalt flakes and preparation method and application thereof

By carrying out sulfonate modification treatment on the basalt scales, the electronegative properties of the surface are increased, the problems of uneven dispersion and poor compatibility are solved, and the coating performance and stability are improved.

CN118307972BActive Publication Date: 2024-10-01JIHUA LAB
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410748517.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-01
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

Basalt flakes are unevenly dispersed in the matrix, resulting in reduced coating performance, poor interface compatibility with the resin, and easy agglomeration and sedimentation.

Method used

By reacting basalt flakes with a silane coupling agent containing thiol groups, thiol-modified basalt flakes are formed, and then reacted with sulfonate to prepare sulfonate-modified basalt flakes, which increases the negative charge on the surface and reduces agglomeration.

Benefits of technology

The uniform dispersion of basalt scales in the matrix is ​​achieved, which improves the overall performance of the coating, enhances its compatibility with resin, and reduces agglomeration and settlement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118307972B_ABST
    Figure CN118307972B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of material technology, specifically to a sulfonate-modified basalt flake and a preparation method and application thereof, comprising: reacting basalt flake with a silane coupling agent containing a mercapto group to prepare a mercapto-modified basalt flake; reacting sulfonate with the mercapto-modified basalt flake under the action of a catalyst to prepare a sulfonate-modified basalt flake. The preparation method of the embodiment of the present invention modifies the surface of the basalt flake by sulfonation so that the surface of the basalt flake carries a sulfonate group; since the sulfonate group carries a negative charge, according to the principle of mutual repulsion of like charges, the basalt flake with the surface sulfonate group modified is not easy to agglomerate, thereby further facilitating its uniform dispersion in the matrix.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material technology, and in particular to a sulfonate-modified basalt flake and a preparation method and application thereof. Background Art

[0002] Basalt flakes are a low-cost, high-performance, low-carbon and environmentally friendly material. Its main components include silica, alumina, iron oxide, calcium oxide, magnesium oxide, sodium oxide, titanium dioxide, etc., among which silica and alumina account for about 50%-60% and 13%-16% respectively.

[0003] Basalt flakes are an inorganic flake material with a certain amount of silanol on the surface, which makes them hydrophilic and oleophobic, and have poor interfacial compatibility with organic resins. At the same time, basalt flakes have a large specific gravity, poor dispersion stability in coatings, uncontrolled arrangement, and are prone to agglomeration and sedimentation, which prevents the basalt flakes from combining ideally with the resin interface, resulting in a decrease in the overall performance of the coating.

[0004] When basalt flakes are added to materials such as ultra-high molecular weight polyethylene, because the matrix is ​​organic and basalt flakes are inorganic, the compatibility between the two is poor. Basalt flakes tend to agglomerate, resulting in uneven dispersion of basalt flakes in the matrix, affecting the lubrication performance.

[0005] Therefore, finding a basalt flake that is conducive to uniform dispersion in the matrix has become a hot topic of current research. Summary of the invention

[0006] In order to solve at least one of the above technical problems, the present invention provides a sulfonate-modified basalt flake, a preparation method and application thereof, by treating the basalt flake so that its surface has negatively charged sulfonate groups, thereby reducing the agglomeration of the basalt flakes.

[0007] As one aspect, the present invention provides a method for preparing sulfonate-modified basalt flakes, comprising: reacting basalt flakes with a silane coupling agent containing a mercapto group to prepare mercapto-modified basalt flakes; reacting sulfonate with mercapto-modified basalt flakes under the action of a catalyst to prepare sulfonate-modified basalt flakes.

[0008] In some embodiments of the present invention, in the step of preparing thiol-modified basalt flakes, the mass ratio of basalt flakes to thiol-containing silane coupling agent is 1:(0.01-10), for example, it can be 1:0.6, 1:1.9, 1:2.7, 1:3.9, 1:4.8, 1:5.4, 1:6.7, 1:7.9, 1:8.7, 1:9.3, 1:9.8, etc.; and / or, the reaction temperature is 80-100°C, for example, it can be 81°C, 84°C, 87°C, 89°C, 93°C, 96°C, 98°C, 99°C, etc.; and / or, the reaction time is 1-5h, for example, it can be 1.3h, 1.8h, 2.1h, 2.6h, 3.3h, 3.9h, 4.3h, 4.7h, 4.9h, etc.

[0009] In some embodiments of the present invention, the mercapto-containing silane coupling agent includes at least one of (3-mercaptopropyl)triethoxysilane and (3-mercaptopropyl)trimethoxysilane.

[0010] In some embodiments of the present invention, in the step of preparing sulfonate-modified basalt flakes, the mass ratio of mercapto-modified basalt flakes, sulfonate, and catalyst is 1:(0.1-1):(0.01-0.2), for example, it can be 1:0.36:0.06, 1:0.45:0.09, 1:0.58:0.12, 1:0.67:0.14, 1:0.76:0.16, 1:0.89:0.18, 1:0.97:0.19, etc.; and / or, the reaction temperature is 110-1 The temperature of the reaction mixture may be 20°C, for example, it may be 111.6°C, 112.8°C, 113.7°C, 114.9°C, 115.8°C, 116.4°C, 117.6°C, 119.8°C, etc.; and / or the reaction time is 1-24h, for example, it may be 1.6h, 3.7h, 5.8h, 7.9h, 9.6h, 11.4h, 13.9h, 15.6h, 16.8h, 17.7h, 18.9h, 21.6h, 23.9h, etc.; and / or the catalyst includes at least one of sodium iodide and potassium iodide.

[0011] In some embodiments of the present invention, the sulfonate is a halogenated hydrocarbon sulfonate.

[0012] In some embodiments of the present invention, the halogenated hydrocarbon sulfonate is sodium 4-chloro-1-hydroxybutane sulfonate.

[0013] In some embodiments of the present invention, the method further includes: treating the basalt flakes with a strong alkaline solution.

[0014] In some embodiments of the present invention, the mass fraction of the strong alkali in the strong alkali solution is 1-40%, for example, it can be 2.3%, 6.8%, 12.9%, 19.8%, 23.7%, 32.8%, 38.9%, etc.; and / or the strong alkali solution includes at least one of a sodium hydroxide aqueous solution and a potassium hydroxide aqueous solution.

[0015] As another aspect, the present invention provides a sulfonate-modified basalt flake obtained by the preparation method of the sulfonate-modified basalt flake as described above.

[0016] As yet another aspect, the present invention provides an application of the sulfonate-modified basalt flakes as described above in polyethylene materials.

[0017] The technical solution of the embodiment of the present invention has the following advantages:

[0018] The preparation method of sulfonate-modified basalt flakes in the embodiment of the present invention is to modify the surface of the basalt flakes by sulfonation so that the surface of the basalt flakes has sulfonate groups; since the sulfonate groups are negatively charged, according to the principle of mutual repulsion of like charges, the basalt flakes with surface sulfonate groups are not easy to agglomerate, which is further conducive to their uniform dispersion in the matrix.

[0019] Specifically, by soaking the basalt flakes in a strong alkali, impurities such as oil in the basalt flakes can be removed, and the alkali solution can etch the surface, so that the surface of the basalt flakes has more hydroxyl groups that can react with the silane coupling agent; the basalt flakes treated with a strong alkali solution are mixed and heated with a silane coupling agent containing a mercapto group in an ethanol solution, so that the silane coupling agent reacts with the basalt flakes, and the silane coupling agent is connected to the surface of the basalt flakes with a silicon-oxygen bond, and the surface of the basalt flakes has a mercapto group, thereby obtaining a mercapto-modified basalt flake; the mercapto-modified basalt flakes undergo a substitution reaction with sulfonates to form carbon-sulfur bonds, and the surface of the basalt flakes has a sulfonate group, and the negative charge of the surface of the basalt flakes is further enhanced. Since charges of the same kind repel each other, the basalt flakes become less likely to agglomerate.

[0020] In addition, the preparation method of the sulfonate-modified basalt flakes of the embodiment of the present invention is simple, feasible and highly operable. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0023] Figure 1 This is a comparison chart of the Zeta potential test results of the sulfonate-modified basalt flakes prepared in Examples 1-3 of the present invention and the basalt flakes prepared in the comparative example;

[0024] Figure 2 A comparison chart of X-ray photoelectron spectroscopy test results of sulfonate-modified basalt flakes prepared in Examples 1-3 of the present invention and basalt flakes prepared in the comparative example;

[0025] Figure 3 It is a partial enlarged view of the comparison diagram of the X-ray photoelectron spectroscopy test results of the sulfonate-modified basalt flakes prepared in Examples 1-3 of the present invention and the basalt flakes prepared in the comparative example. DETAILED DESCRIPTION

[0026] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0027] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.

[0028] According to an embodiment of one aspect of the present invention, a method for preparing sulfonate-modified basalt flakes is provided, comprising: reacting basalt flakes with a silane coupling agent containing a mercapto group to prepare mercapto-modified basalt flakes; reacting sulfonate with mercapto-modified basalt flakes under the action of a catalyst to prepare sulfonate-modified basalt flakes.

[0029] The preparation method of sulfonate-modified basalt flakes of the embodiment of the present invention is as follows: basalt flakes and a silane coupling agent containing a mercapto group are mixed and heated in ethanol, so that the silane coupling agent reacts with the hydroxyl groups on the surface of the basalt flakes, and the silane coupling agent is connected to the surface of the basalt flakes by a silicon-oxygen bond, and the surface of the basalt flakes has a mercapto group, thereby preparing mercapto-modified basalt flakes; the mercapto-modified basalt flakes are substituted with sulfonates to form carbon-sulfur bonds, and the surface of the basalt flakes has a sulfonate group, and the negative charge of the surface of the basalt flakes is further enhanced. Since charges of the same kind repel each other, the basalt flakes become less likely to agglomerate.

[0030] In some embodiments of the present invention, a method for preparing sulfonate-modified basalt flakes comprises the following steps:

[0031] (1) Basalt flakes are soaked in a strong alkaline solution for a certain period of time.

[0032] (2) Separate the soaked basalt flakes from the strong alkaline solution and wash them with water until the pH value of the solution after the last wash is 6.8-7.2.

[0033] (3) Dry the cleaned basalt flakes thoroughly in an oven.

[0034] (4) Weigh a certain amount of dried basalt flakes, add them to ethanol, and then add a certain amount of silane coupling agent with a mercapto group. While stirring, heat until the ethanol boils, keep heating for a certain period of time, and condense the volatilized ethanol and reflux it into the mixed solution.

[0035] (5) Separate the basalt flakes from the ethanol and wash them repeatedly with water or ethanol.

[0036] (6) Dry the cleaned basalt flakes thoroughly in an oven.

[0037] (7) Take a certain amount of sodium iodide, potassium carbonate, and sodium 4-chloro-1-hydroxybutane sulfonate and dry them thoroughly in an oven.

[0038] (8) Weigh a certain amount of the above-mentioned basalt flakes and dried sodium iodide, potassium carbonate, and sodium 4-chloro-1-hydroxybutane sulfonate, add them to dimethyl sulfoxide, and stir evenly.

[0039] (9) Under the continuous protection of inert gas, heat the above mixed solution to 110-120°C and keep it warm for a certain period of time.

[0040] (10) The treated basalt flakes are separated from the mixed solution and washed repeatedly with water and ethanol.

[0041] (11) The cleaned basalt flakes are fully dried in an oven to obtain basalt flakes having sulfonate groups on the surface.

[0042] In some embodiments of the present invention, in step (1), the strong alkali solution used is an aqueous solution of sodium hydroxide or potassium hydroxide, and the concentration is 1-40% by mass fraction, for example, 2.3%, 9.3%, 12.4%, 21.9%, 29.6%, 32.1%, 36.3%, 39.1%, 39.8%, etc. The basalt flakes are powders with a particle size of 100-1000 mesh, for example, 109 mesh, 226 mesh, 378 mesh, 439 mesh, 589 mesh, 672 mesh, 768 mesh, 839 mesh, 987 mesh, etc. The mass ratio of basalt flakes to the strong alkali solution is 1:10-1:100, for example, 1:12, 1:23, 1:36, 1:41, 1:49, 1:58, 1:68, 1:76, 1:86, 1:98, etc. The immersion time is 1-10 hours, for example, it can be 1.3 hours, 2.4 hours, 3.6 hours, 4.7 hours, 5.6 hours, 6.4 hours, 7.3 hours, 8.4 hours, 9.2 hours, 9.8 hours, etc. During the immersion process, mechanical stirring with a stirring paddle, stirring with a magnetic stirring bar or ultrasonic oscillation are used to keep the solution uniform.

[0043] In some embodiments of the present invention, in step (2), the separation method can be one or any combination of filter paper filtration, filter cloth filtration or centrifugal separation. The water used for washing can be deionized water or distilled water. The number of washing times is 3 to 10 times.

[0044] In some embodiments of the present invention, in step (3), the oven used can be a forced air drying oven or a vacuum drying oven, the drying temperature is 90-170°C, for example, 92°C, 98°C, 102°C, 112°C, 121°C, 134°C, 141°C, 153°C, 164°C, etc., and the drying time is 1-10h, for example, it can be 1.8h, 2.3h, 3.1h, 3.9h, 4.8h, 5.6h, 6.7h, 7.8h, 8.4h, 9.8h, etc.

[0045] In some embodiments of the present invention, in step (4), the ethanol used is anhydrous ethanol or ethanol with a water content of no more than 2%, and the ratio of the amount of ethanol to the amount of basalt flakes can be 20 mL ethanol / 1 g basalt flakes to 300 mL ethanol / 1 g basalt flakes, for example, 26 mL ethanol / 1 g basalt flakes, 34 mL ethanol / 1 g basalt flakes, 48 ​​mL ethanol / 1 g basalt flakes, 68 mL ethanol / 1 g basalt flakes, 89 mL ethanol / 1 g basalt flakes, 103 mL ethanol / 1 g basalt flakes, Scales, 126mL ethanol / 1g basalt scales, 149mL ethanol / 1g basalt scales, 167mL ethanol / 1g basalt scales, 196mL ethanol / 1g basalt scales, 229mL ethanol / 1g basalt scales, 257mL ethanol / 1g basalt scales, 279mL ethanol / 1g basalt scales, 297mL ethanol / 1g basalt scales, etc.; the silane coupling agent with mercapto group used can be (3-mercaptopropyl)triethoxysilane, (3-mercaptopropyl)trimethoxysilane or other silane coupling agents with mercapto group. The purity of the silane coupling agent can be 90-98%, and the concentration of the silane coupling agent with a mercapto group in ethanol can be 0.1-5% by mass, for example, 0.65%, 1.03%, 1.93%, 2.43%, 2.87%, 3.23%, 3.83%, 4.26%, 4.63%, 4.89%, etc. The heating temperature is 80-100°C, for example, 81°C, 86°C, 89°C, 93°C, 96°C, 98°C, etc. The heating time is 1-5h, for example, 1.3h, 1.8h, 2.1h, 2.6h, 2.9h, 3.3h, 3.7h, 3.9h, 4.3h, 4.8h, etc. The stirring method is mechanical stirring with a stirring paddle or stirring with a magnetic stirring bar.

[0046] In some embodiments of the present invention, in step (5), the separation method can be one or any combination of filter paper filtration, filter cloth filtration or centrifugal separation. The water used for washing can be deionized water or distilled water, and the ethanol used can be anhydrous ethanol or ethanol with a water content of no more than 25%. The number of washing times is 3 to 10 times.

[0047] In some embodiments of the present invention, in step (6), the oven used can be a forced air drying oven or a vacuum drying oven, and the drying temperature is 90-110°C, for example, it can be 91°C, 94°C, 98°C, 101°C, 106°C, 109°C, etc.; the drying time is 1-10h, for example, it can be 1.8h, 2.3h, 3.6h, 4.2h, 5.3h, 6.9h, 7.8h, 8.6h, 9.3h, etc.

[0048] In some embodiments of the present invention, in step (7), the oven used can be a forced air drying oven or a vacuum drying oven, and the drying temperature is 30-100°C, for example, it can be 32°C, 46°C, 58°C, 64°C, 76°C, 87°C, 92°C, 98°C, etc.; the drying time is 1-10h, for example, it can be 1.9h, 2.4h, 3.7h, 4.3h, 5.4h, 6.8h, 7.9h, 8.7h, 9.6h, etc.

[0049] In some embodiments of the present invention, in step (8), based on the mass of the added basalt flakes as 1 part, the amount of sodium 4-chloro-1-hydroxybutane sulfonate is 0.1 to 1 part, for example, it can be 0.12 parts, 0.26 parts, 0.39 parts, 0.41 parts, 0.53 parts, 0.61 parts, 0.78 parts, 0.83 parts, 0.91 parts, 0.98 parts, etc.; the amount of sodium iodide is 0.01 to 0.2 parts, for example, it can be 0.03 parts, 0.06 parts, 0.09 parts, 0.10 parts, 0.11 parts, 0.12 parts, 0.26 parts, 0.39 parts, 0.41 parts, 0.53 parts, 0.61 parts, 0.78 parts, 0.83 parts, 0.91 parts, 0.98 parts, etc. .11 parts, 0.13 parts, 0.16 parts, 0.17 parts, 0.18 parts, 0.19 parts, etc.; the amount of potassium carbonate is 1 part to 5 parts, for example, it can be 1.1 parts, 2.3 parts, 3.1 parts, 3.9 parts, 4.3 parts, 4.9 parts, etc.; the amount of dimethyl sulfoxide is 50 parts to 300 parts, for example, it can be 56 parts, 67 parts, 86 parts, 97 parts, 126 parts, 151 parts, 179 parts, 198 parts, 226 parts, 258 parts, 278 parts, 289 parts, 298 parts, etc. Sodium 4-chloro-1-hydroxybutane sulfonate can be replaced by a derivative containing halogen and sulfonate. Potassium carbonate can be replaced by sodium carbonate. Sodium iodide can be replaced by potassium iodide. Among them, potassium carbonate or sodium carbonate is a promoter; sodium iodide or potassium iodide is a catalyst. The purity of sodium 4-chloro-1-hydroxybutane sulfonate, sodium iodide and potassium carbonate are all analytical grade, and the purity of dimethyl sulfoxide is anhydrous solvent grade.

[0050] In some embodiments of the present invention, in step (9), the inert gas used is nitrogen or argon, and the gas flow rate is 10-100 mL / min; the heating time is 1-24 h, for example, it can be 1.6 h, 2.8 h, 3.6 h, 4.8 h, 5.6 h, 6.7 h, 8.6 h, 9.6 h, 12.6 h, 13.9 h, 16.8 h, 18.9 h, 21.6 h, 23.8 h, etc.; the heating temperature of the mixed solution is 110-120 ° C; for example, it can be 111.3 ° C, 112.6 ° C, 113.8 ° C, 114.7 ° C, 116.8 ° C, 117.2 ° C, 118.9 ° C, 119.8 ° C, etc.

[0051] In some embodiments of the present invention, in step (10), the separation method can be one or any combination of filter paper filtration, filter cloth filtration or centrifugal separation. The water used for washing can be deionized water or distilled water, and the ethanol used can be anhydrous ethanol or ethanol with a water content of no more than 25%.

[0052] In some embodiments of the present invention, in step (11), the oven used can be a forced air drying oven or a vacuum drying oven, and the drying temperature is 90-110°C, for example, it can be 93°C, 96°C, 98°C, 101°C, 104°C, 106°C, 109°C, etc.; the drying time is 1-10h, for example, it can be 1.6h, 2.9h, 3.7h, 4.6h, 5.6h, 6.8h, 7.4h, 8.6h, 9.8h, etc.

[0053] In order to further illustrate the effect of the present invention, specific embodiments are used for illustration below.

[0054] Example 1

[0055] Preparation of sulfonate-modified basalt flakes

[0056] (1) Weigh 32 g of 240-mesh basalt flakes and soak them in 10% sodium hydroxide solution for 4 hours.

[0057] (2) Filter the soaked basalt flakes from the sodium hydroxide solution and wash them with water until the pH value of the solution obtained by the last washing is 7.

[0058] (3) Dry the washed basalt flakes in a forced air drying oven at 100°C for 6 hours.

[0059] (4) Weigh 6 g of dried basalt flakes and add them to 300 mL of ethanol, then add 1.8 g of (3-mercaptopropyl)triethoxysilane (purity 98%). Heat to 90°C while stirring, keep warm for 4 hours, and condense the volatilized ethanol and reflux it into the mixed solution.

[0060] (5) Separate the basalt scales from the ethanol and wash them repeatedly with water or ethanol for 5 times.

[0061] (6) Dry the cleaned basalt flakes in an oven at 100°C for 5 hours.

[0062] (7) Take a certain amount of sodium iodide, potassium carbonate, and sodium 4-chloro-1-hydroxybutane sulfonate and dry them thoroughly in an oven at 50°C.

[0063] (8) Weigh 1 g of basalt flakes, 0.03 g of sodium iodide, 2 g of potassium carbonate, and 0.25 g of sodium 4-chloro-1-hydroxybutane sulfonate, add them to 300 mL of dimethyl sulfoxide, and stir evenly;

[0064] (9) Under the continuous protection of nitrogen gas, heat the above mixed solution to 120°C and keep it warm for 12 hours.

[0065] (10) The treated basalt flakes were separated from the mixed solution and washed repeatedly with water and ethanol for 5 times.

[0066] (11) The cleaned basalt flakes are fully dried in a forced air drying oven at 100° C. to obtain basalt flakes having sulfonate groups on the surface.

[0067] Example 2

[0068] Preparation of sulfonate-modified basalt flakes

[0069] (1) Weigh 32 g of 240-mesh basalt flakes and soak them in 10% sodium hydroxide solution for 4 hours.

[0070] (2) Filter the soaked basalt flakes from the sodium hydroxide solution and wash them with water until the pH value of the solution obtained by the last washing is 7.

[0071] (3) Dry the washed basalt flakes in a forced air drying oven at 100°C for 6 hours.

[0072] (4) Weigh 6 g of dried basalt flakes and add them to 300 mL of ethanol, then add 1.8 g of (3-mercaptopropyl)triethoxysilane (purity 98%). Heat to 90°C while stirring, keep warm for 4 hours, and condense the volatilized ethanol and reflux it into the mixed solution.

[0073] (5) Separate the basalt scales from the ethanol and wash them repeatedly with water or ethanol for 5 times.

[0074] (6) Dry the cleaned basalt flakes in an oven at 100°C for 5 hours.

[0075] (7) Take a certain amount of sodium iodide, potassium carbonate, and sodium 4-chloro-1-hydroxybutane sulfonate and dry them thoroughly in an oven at 50°C.

[0076] (8) Weigh 1 g of basalt flakes, 0.2 g of sodium iodide, 8 g of sodium carbonate, and 1 g of sodium 4-chloro-1-hydroxybutane sulfonate, add them to 300 mL of dimethyl sulfoxide, and stir evenly;

[0077] (9) Under the continuous protection of nitrogen gas, heat the above mixed solution to 110°C and keep it warm for 24 hours.

[0078] (10) The treated basalt flakes were separated from the mixed solution and washed repeatedly with water and ethanol for 5 times.

[0079] (11) The cleaned basalt flakes are fully dried in a forced air drying oven at 100° C. to obtain basalt flakes having sulfonate groups on the surface.

[0080] Example 3

[0081] Preparation of sulfonate-modified basalt flakes

[0082] (1) Weigh 32 g of 240-mesh basalt flakes and soak them in 10% sodium hydroxide solution for 4 hours.

[0083] (2) Filter the soaked basalt flakes from the sodium hydroxide solution and wash them with water until the pH value of the solution obtained by the last washing is 7.

[0084] (3) Dry the washed basalt flakes in a forced air drying oven at 100°C for 6 hours.

[0085] (4) Weigh 6 g of dried basalt flakes and add them to 300 mL of ethanol, then add 1.8 g of (3-mercaptopropyl)triethoxysilane (purity 98%). Heat to 90°C while stirring, keep warm for 4 hours, and condense the volatilized ethanol and reflux it into the mixed solution.

[0086] (5) Separate the basalt scales from the ethanol and wash them repeatedly with water or ethanol for 5 times.

[0087] (6) Dry the cleaned basalt flakes in an oven at 100°C for 5 hours.

[0088] (7) Take a certain amount of sodium iodide, potassium carbonate, and sodium 4-chloro-1-hydroxybutane sulfonate and dry them thoroughly in an oven at 50°C.

[0089] (8) Weigh 1 g of basalt flakes, 0.01 g of potassium iodide, 0.8 g of potassium carbonate, and 0.1 g of sodium 4-chloro-1-hydroxybutane sulfonate, add them to 300 mL of dimethyl sulfoxide, and stir evenly;

[0090] (9) Under the continuous protection of nitrogen gas, heat the above mixed solution to 120°C and keep it warm for 1 hour.

[0091] (10) The treated basalt flakes were separated from the mixed solution and washed repeatedly with water and ethanol for 5 times.

[0092] (11) The cleaned basalt flakes are fully dried in a forced air drying oven at 100° C. to obtain basalt flakes having sulfonate groups on the surface.

[0093] Comparative Example

[0094] (1) Weigh 32 g of 240-mesh basalt flakes and soak them in 10% sodium hydroxide solution for 4 hours.

[0095] (2) Filter the soaked basalt flakes from the sodium hydroxide solution and wash them with water until the pH value of the solution obtained by the last washing is 7.

[0096] (3) Dry the washed basalt flakes in a forced air drying oven at 100°C for 6 hours.

[0097] (4) Weigh 6 g of dried basalt flakes.

[0098] (5) Separate the basalt scales from the ethanol and wash them repeatedly with water or ethanol for 5 times.

[0099] (6) Dry the cleaned basalt flakes in an oven at 100°C for 5 hours.

[0100] Performance Characterization

[0101] The basalt flakes of Examples 1-3 and the comparative example were characterized respectively, and the test results are as follows:

[0102] (1) The Zeta potential test results of the sulfonate-modified basalt flakes prepared in Examples 1-3 and the basalt flakes prepared in the comparative example are shown in the figure below: Figure 1 The peak value of the Zeta potential test result curve corresponds to the positive and negative values ​​of the Zeta potential, which reflects the charge of the sample particles. The larger the absolute value of the Zeta potential, the greater the repulsive force between the particles, and the stronger the ability of the particles to resist aggregation. Figure 1 From the data analysis, it can be seen that the Zeta potential of the test peak of the sulfonate modified basalt scale prepared in Example 1 is -23.2, the Zeta potential of the test peak of the sulfonate modified basalt scale prepared in Example 2 is -22.5, the Zeta potential of the test peak of the sulfonate modified basalt scale prepared in Example 3 is -22, and the Zeta potential of the test peak of the comparative example is -21.5. The sulfonate modified basalt scale prepared in each example has a stronger tendency to disperse in water or other solutions.

[0103] (2) Figure 3 for Figure 2 A comparison of the partial enlarged images of Figure 2 , Figure 3 It can be seen that sulfur was detected in the basalt flakes prepared in Examples 1, 2, and 3, and there were two sulfur elements in different chemical states (there were two peaks in the X-ray photoelectron energy spectrum curve), while no sulfur was detected in the basalt flakes prepared in the comparative example.

[0104] In summary, the method for preparing sulfonate-modified basalt flakes of the embodiment of the present invention is to mix and heat basalt flakes with a silane coupling agent containing a mercapto group in ethanol, so that the silane coupling agent reacts with the hydroxyl groups on the surface of the basalt flakes, and the silane coupling agent is connected to the surface of the basalt flakes by a silicon-oxygen bond, and the surface of the basalt flakes has a mercapto group, thereby preparing mercapto-modified basalt flakes; the mercapto-modified basalt flakes are substituted with sulfonates to form carbon-sulfur bonds, and the surface of the basalt flakes has a sulfonate group, and the negative charge of the surface of the basalt flakes is further enhanced. Since charges of the same kind repel each other, the basalt flakes become less likely to agglomerate.

[0105] It should be noted that, in this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.

[0106] The above description is only a specific embodiment of the present invention, so that those skilled in the art can understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments described herein, but should conform to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing sulfonate-modified basalt flakes, include: The basalt flakes are reacted with a silane coupling agent containing a mercapto group to prepare mercapto-modified basalt flakes; Under the action of a catalyst, the halogenated hydrocarbon sulfonate undergoes a substitution reaction with the mercapto-modified basalt flakes to form a carbon-sulfur bond, thereby preparing sulfonate-modified basalt flakes.

2. The preparation method according to claim 1, It is characterized in that In the step of preparing mercapto-modified basalt flakes, The mass ratio of the basalt flakes to the silane coupling agent containing a mercapto group is 1:(0.01-10); and / or, the reaction temperature is 80-100°C; And / or, the reaction time is 1-5h.

3. The preparation method according to claim 2, It is characterized in that The mercapto-containing silane coupling agent includes at least one of (3-mercaptopropyl)triethoxysilane and (3-mercaptopropyl)trimethoxysilane.

4. The preparation method according to claim 3, It is characterized in that In the step of preparing sulfonate-modified basalt flakes, The mass ratio of the mercapto-modified basalt flakes, sulfonate and catalyst is 1:(0.1-1):(0.01-0.2); and / or, the reaction temperature is 110-120°C; and / or, the reaction time is 1-24h; And / or, the catalyst includes at least one of sodium iodide and potassium iodide.

5. The preparation method according to claim 1, It is characterized in that The halogenated hydrocarbon sulfonate is sodium 4-chloro-1-hydroxybutane sulfonate.

6. The preparation method according to claim 5, It is characterized in that Also includes: The basalt flakes are treated with a strong alkaline solution.

7. The preparation method according to claim 6, It is characterized in that In the strong alkali solution, the mass fraction of the strong alkali is 1-40%; And / or, the strong alkaline solution includes at least one of a sodium hydroxide aqueous solution and a potassium hydroxide aqueous solution.

8. Sulfonate-modified basalt flakes obtained by the preparation method of sulfonate-modified basalt flakes as described in any one of claims 1 to 7.

9. Use of the sulfonate-modified basalt flakes as claimed in claim 8 in polyethylene materials.